MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Sandvik Kanthal D Resistance Wire
Categories: Metal; Ferrous Metal; Ferritic; Superalloy; Iron Base

Material Notes: Kanthal D is a ferritic iron-chromium-aluminium alloy (FeCrAl alloy) for use at temperatures up to 1300°C (2370°F). The alloy is characterized by high resistivity and good oxidation resistance. Kanthal D is used in home appliances and industrial furnaces. Typical applications in home appliances include metal sheathed tubular elements for dishwashers, elements embedded in ceramics for panel heaters, cartridge elements in metal dies, heating cables and rope heaters in defrosting and deicing elements, mica elements used in irons, quartz tube heaters for space heating, industrial infrared dryers, in coils on molded ceramic fibre for boiling plates with ceramic hobs, in bead insulated coils for panel heaters, in suspended coil elements for air heaters in laundry dryers. In industrial applications Kanthal D is used in, for example, terminals to furnace elements, porcupine elements for air heating, and in furnace heating elements.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.25 g/cc0.262 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers  230
@Thickness 1.00 mm
230
@Thickness 0.0394 in
 230
@Thickness 4.00 mm
230
@Thickness 0.157 in
Tensile Strength, Ultimate 34.0 MPa
@Temperature 900 °C
4930 psi
@Temperature 1650 °F
deformation rate= 6.2x10-2/min
 650 MPa
@Thickness 4.00 mm
94300 psi
@Thickness 0.157 in
 670 MPa
@Thickness 1.00 mm
97200 psi
@Thickness 0.0394 in
Tensile Strength, Yield  450 MPa
@Strain 0.2 %,
Thickness 4.00 mm
65300 psi
@Strain 0.2 %,
Thickness 0.157 in
 485 MPa
@Strain 0.2 %,
Thickness 1.00 mm
70300 psi
@Strain 0.2 %,
Thickness 0.0394 in
Elongation at Break  18 %
@Thickness 4.00 mm
18 %
@Thickness 0.157 in
 23 %
@Thickness 1.00 mm
23 %
@Thickness 0.0394 in
Creep Strength  0.500 MPa
@Temperature 1000 °C,
Time 3.60e+6 sec
72.5 psi
@Temperature 1830 °F,
Time 1000 hour
1% elongation
 1.20 MPa
@Temperature 800 °C,
Time 3.60e+6 sec
174 psi
@Temperature 1470 °F,
Time 1000 hour
1% elongation
Modulus of Elasticity 220 GPa31900 ksi
 130 GPa
@Temperature 1000 °C
18900 ksi
@Temperature 1830 °F
 150 GPa
@Temperature 800 °C
21800 ksi
@Temperature 1470 °F
 170 GPa
@Temperature 600 °C
24700 ksi
@Temperature 1110 °F
 190 GPa
@Temperature 400 °C
27600 ksi
@Temperature 752 °F
 205 GPa
@Temperature 200 °C
29700 ksi
@Temperature 392 °F
 210 GPa
@Temperature 100 °C
30500 ksi
@Temperature 212 °F
Poissons Ratio 0.300.30
Shear Modulus 85.0 GPa12300 ksicalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000135 ohm-cm0.000135 ohm-cm
 0.00000146 ohm-cm
@Temperature 1200 °C
0.00000146 ohm-cm
@Temperature 2190 °F
 0.00000146 ohm-cm
@Temperature 1300 °C
0.00000146 ohm-cm
@Temperature 2370 °F
 0.000135 ohm-cm
@Temperature 100 °C
0.000135 ohm-cm
@Temperature 212 °F
 0.000136 ohm-cm
@Temperature 200 °C
0.000136 ohm-cm
@Temperature 392 °F
 0.000136 ohm-cm
@Temperature 300 °C
0.000136 ohm-cm
@Temperature 572 °F
 0.000137 ohm-cm
@Temperature 400 °C
0.000137 ohm-cm
@Temperature 752 °F
 0.000139 ohm-cm
@Temperature 500 °C
0.000139 ohm-cm
@Temperature 932 °F
 0.000140 ohm-cm
@Temperature 600 °C
0.000140 ohm-cm
@Temperature 1110 °F
 0.000141 ohm-cm
@Temperature 700 °C
0.000141 ohm-cm
@Temperature 1290 °F
 0.000143 ohm-cm
@Temperature 800 °C
0.000143 ohm-cm
@Temperature 1470 °F
 0.000144 ohm-cm
@Temperature 900 °C
0.000144 ohm-cm
@Temperature 1650 °F
 0.000144 ohm-cm
@Temperature 1000 °C
0.000144 ohm-cm
@Temperature 1830 °F
 0.000144 ohm-cm
@Temperature 1100 °C
0.000144 ohm-cm
@Temperature 2010 °F
Curie Temperature 600 °C1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.0 µm/m-°C
@Temperature 20.0 - 250 °C
6.11 µin/in-°F
@Temperature 68.0 - 482 °F
 12.0 µm/m-°C
@Temperature 20.0 - 500 °C
6.67 µin/in-°F
@Temperature 68.0 - 932 °F
 14.0 µm/m-°C
@Temperature 20.0 - 750 °C
7.78 µin/in-°F
@Temperature 68.0 - 1380 °F
 15.0 µm/m-°C
@Temperature 20.0 - 1000 °C
8.33 µin/in-°F
@Temperature 68.0 - 1830 °F
Specific Heat Capacity  0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
 0.560 J/g-°C
@Temperature 200 °C
0.134 BTU/lb-°F
@Temperature 392 °F
 0.630 J/g-°C
@Temperature 400 °C
0.151 BTU/lb-°F
@Temperature 752 °F
 0.710 J/g-°C
@Temperature 800 °C
0.170 BTU/lb-°F
@Temperature 1470 °F
 0.720 J/g-°C
@Temperature 1000 °C
0.172 BTU/lb-°F
@Temperature 1830 °F
 0.740 J/g-°C
@Temperature 1200 °C
0.177 BTU/lb-°F
@Temperature 2190 °F
 0.750 J/g-°C
@Temperature 600 °C
0.179 BTU/lb-°F
@Temperature 1110 °F
Thermal Conductivity  11.0 W/m-K
@Temperature 50.0 °C
76.3 BTU-in/hr-ft²-°F
@Temperature 122 °F
 20.0 W/m-K
@Temperature 600 °C
139 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.0 W/m-K
@Temperature 800 °C
153 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 26.0 W/m-K
@Temperature 1000 °C
180 BTU-in/hr-ft²-°F
@Temperature 1830 °F
 27.0 W/m-K
@Temperature 1200 °C
187 BTU-in/hr-ft²-°F
@Temperature 2190 °F
Melting Point 1500 °C2730 °F
Maximum Service Temperature, Air 1300 °C2370 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.700.70fully oxidized
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 4.8 %4.8 %
Carbon, C <= 0.080 %<= 0.080 %
Chromium, Cr 20.5 - 23.5 %20.5 - 23.5 %
Iron, Fe >= 70.42 %>= 70.42 %
Manganese, Mn <= 0.50 %<= 0.50 %
Silicon, Si <= 0.70 %<= 0.70 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Sandvik Kanthal D Resistance Ribbon
Sandvik Kanthal A-1 Resistance Wire
Sandvik Kanthal AF Resistance Wire
Aluminum 6063-O
302 Stainless Steel, annealed bar

NSANDV065a / 171819

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.