MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik Kanthal D Resistance Wire
Categories: Metal; Ferrous Metal; Ferritic; Superalloy; Iron Base

Material Notes: Kanthal D is a ferritic iron-chromium-aluminium alloy (FeCrAl alloy) for use at temperatures up to 1300°C (2370°F). The alloy is characterized by high resistivity and good oxidation resistance. Kanthal D is used in home appliances and industrial furnaces. Typical applications in home appliances include metal sheathed tubular elements for dishwashers, elements embedded in ceramics for panel heaters, cartridge elements in metal dies, heating cables and rope heaters in defrosting and deicing elements, mica elements used in irons, quartz tube heaters for space heating, industrial infrared dryers, in coils on molded ceramic fibre for boiling plates with ceramic hobs, in bead insulated coils for panel heaters, in suspended coil elements for air heaters in laundry dryers. In industrial applications Kanthal D is used in, for example, terminals to furnace elements, porcupine elements for air heating, and in furnace heating elements.

Information provided by Sandvik

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.25 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 230
@Thickness 1.00 mm
 230
@Thickness 4.00 mm
Tensile Strength, Ultimate 34.0 MPa
@Temperature 900 °C
deformation rate= 6.2x10-2/min
 650 MPa
@Thickness 4.00 mm
 670 MPa
@Thickness 1.00 mm
Tensile Strength, Yield 450 MPa
@Strain 0.2 %,
Thickness 4.00 mm
 485 MPa
@Strain 0.2 %,
Thickness 1.00 mm
Elongation at Break 18 %
@Thickness 4.00 mm
 23 %
@Thickness 1.00 mm
Creep Strength 0.500 MPa
@Temperature 1000 °C,
Time 3.60e+6 sec
1% elongation
 1.20 MPa
@Temperature 800 °C,
Time 3.60e+6 sec
1% elongation
Modulus of Elasticity 220 GPa
 130 GPa
@Temperature 1000 °C
 150 GPa
@Temperature 800 °C
 170 GPa
@Temperature 600 °C
 190 GPa
@Temperature 400 °C
 205 GPa
@Temperature 200 °C
 210 GPa
@Temperature 100 °C
Poissons Ratio 0.30
Shear Modulus 85.0 GPacalculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000135 ohm-cm
 0.00000146 ohm-cm
@Temperature 1200 °C
 0.00000146 ohm-cm
@Temperature 1300 °C
 0.000135 ohm-cm
@Temperature 100 °C
 0.000136 ohm-cm
@Temperature 200 °C
 0.000136 ohm-cm
@Temperature 300 °C
 0.000137 ohm-cm
@Temperature 400 °C
 0.000139 ohm-cm
@Temperature 500 °C
 0.000140 ohm-cm
@Temperature 600 °C
 0.000141 ohm-cm
@Temperature 700 °C
 0.000143 ohm-cm
@Temperature 800 °C
 0.000144 ohm-cm
@Temperature 900 °C
 0.000144 ohm-cm
@Temperature 1000 °C
 0.000144 ohm-cm
@Temperature 1100 °C
Curie Temperature 600 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.0 µm/m-°C
@Temperature 20.0 - 250 °C
 12.0 µm/m-°C
@Temperature 20.0 - 500 °C
 14.0 µm/m-°C
@Temperature 20.0 - 750 °C
 15.0 µm/m-°C
@Temperature 20.0 - 1000 °C
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
 0.560 J/g-°C
@Temperature 200 °C
 0.630 J/g-°C
@Temperature 400 °C
 0.710 J/g-°C
@Temperature 800 °C
 0.720 J/g-°C
@Temperature 1000 °C
 0.740 J/g-°C
@Temperature 1200 °C
 0.750 J/g-°C
@Temperature 600 °C
Thermal Conductivity 11.0 W/m-K
@Temperature 50.0 °C
 20.0 W/m-K
@Temperature 600 °C
 22.0 W/m-K
@Temperature 800 °C
 26.0 W/m-K
@Temperature 1000 °C
 27.0 W/m-K
@Temperature 1200 °C
Melting Point 1500 °C
Maximum Service Temperature, Air 1300 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.70fully oxidized
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 4.8 %
Carbon, C <= 0.080 %
Chromium, Cr 20.5 - 23.5 %
Iron, Fe >= 70.42 %
Manganese, Mn <= 0.50 %
Silicon, Si <= 0.70 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sandvik Kanthal D Resistance Ribbon
Sandvik Kanthal A-1 Resistance Wire
Sandvik Kanthal AF Resistance Wire
Aluminum 6063-O
302 Stainless Steel, annealed bar

NSANDV065a / 171819

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.