MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Monprene® SP-14966 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Monprene SP-14966 is a high performance thermoplastic elastomer designed for a variety of consumer applications including water sporting goods. Monprene SP-14966 is a translucent, medium hardness, low density, UV resistant, high flow grade that is designed for injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Good Adhesion; Good Colorability; Good Flexibility; Good Moldability; Good Toughness; High Flow; Low Density; Low Specific Gravity; Medium Hardness; Moisture Resistant; Resilient; UV Resistant; Wear Resistant; Without Fillers

Uses: Consumer Applications; Flexible Grips; Gaskets; Grommets; Handles; Plugs; Rubber Replacement; Soft Touch Applications; Sporting Goods; Swimming Pools; Water Sports Equipment; Writing Instruments

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.890 g/cc0.0322 lb/in³ASTM D792
Melt Flow 27 g/10 min
@Load 5.00 kg,
Temperature 200 °C
27 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7070ASTM D2240
 68
@Time 5.00 sec
68
@Time 0.00139 hour
ASTM D2240
Tensile Strength at Break 11.9 MPa1730 psiFlow; ASTM D412
Tensile Stress at Strain  3.62 MPa
@Strain 100 %
525 psi
@Strain 100 %
ASTM D412
 5.34 MPa
@Strain 300 %
775 psi
@Strain 300 %
Flow; ASTM D412
Elongation at Break 700 %700 %Flow; ASTM D412
 
Processing PropertiesMetricEnglishComments
Processing Temperature 199 - 249 °C390 - 480 °FMelt, Injection
Rear Barrel Temperature 182 - 232 °C360 - 450 °FInjection
Middle Barrel Temperature 188 - 238 °C370 - 460 °FInjection
Front Barrel Temperature 193 - 243 °C380 - 470 °FInjection
Nozzle Temperature 199 - 249 °C390 - 480 °FInjection
Zone 1 182 - 232 °C360 - 450 °FExtrusion
Zone 2 188 - 238 °C370 - 460 °FExtrusion
Zone 3 193 - 243 °C380 - 470 °FExtrusion
Zone 4 193 - 243 °C380 - 470 °FExtrusion
Zone 5 199 - 249 °C390 - 480 °FExtrusion
Die Temperature 199 - 249 °C390 - 480 °FExtrusion
Mold Temperature 35.0 - 48.9 °C95.0 - 120 °FInjection
Injection Pressure 1.38 - 5.52 MPa200 - 800 psiInjection
Back Pressure 0.172 - 0.689 MPa25.0 - 100 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpm30 - 100 rpmExtrusion
 50 - 100 rpm50 - 100 rpmInjection
 
Descriptive Properties
AppearanceNatural Color
 Translucent

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Monprene® SP-16920 XRD2 Thermoplastic Elastomer
Lanxess Mesamoll® Plastic Additive
Lanxess Mesamoll® II Plastic Additive
Teknor Apex Monprene® SP-14986 XRD1 Thermoplastic Elastomer
Teknor Apex Monprene® SP-14077 Thermoplastic Elastomer

PTEKNQ0959 / 237450

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.