System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Amco PRIMATOP PP CO 200 NB Impact Polypropylene Copolymer
Categories:
Polymer
;
Thermoplastic
;
Polypropylene (PP)
;
Polypropylene Copolymer
Material Notes:
PP CO 200 NB is cold temperature impact resistant, heat stabilized, and nucleated. Applications include toys and consumer products.
Former A-Top Polymers product; part of Amco product line since 2013.
Key Words:
FDA 21CFR177.1520
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
0.900
g/cc
0.0325
lb/in³
ASTM D1505
Melt Index of Compound
20
g/10 min
@Load 2.16 kg,
Temperature 230 °C
20
g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Hardness, Rockwell R
80
80
ASTM D785
Tensile Strength, Yield
22.1
MPa
3200
psi
2 in/min; ASTM D638
Flexural Modulus
1.07
GPa
155
ksi
0.5 in/min, Tangent Method; ASTM D790
Izod Impact, Notched
0.374
J/cm
@Temperature -30.0 °C
0.700
ft-lb/in
@Temperature -22.0 °F
ASTM D256
0.801
J/cm
@Temperature 0.000 °C
1.50
ft-lb/in
@Temperature 32.0 °F
ASTM D256
NB
@Temperature 22.8 °C
NB
@Temperature 73.0 °F
ASTM D256
Falling Dart Impact
28.2
J
@Temperature -30.0 °C
20.8
ft-lb
@Temperature -22.0 °F
0.5" Tup, 150"/sec; ASTM D3763
Thermal Properties
Metric
English
Comments
Deflection Temperature at 0.46 MPa (66 psi)
79.4
°C
175
°F
ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)
43.3
°C
110
°F
ASTM D648
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Borealis HH450MO Polypropylene
Borealis Borcoat™ GA700E-7032 Syntactic Polypropylene for Steel Pipe Coating
Braskem H362-09RS Cast Film Polypropylene
Aclo Accutech Polypropylene Homopolymer HP0339C30L1 Calcium Reinforced
Overview of materials for Polypropylene with 50% Glass Fiber Filler
PATOP029 / 79972
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
info@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.