MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Eastman 9921W PET Film  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), Unreinforced

Material Notes: Voridian PET 9921W is a copolymer PET. Typical applications include containers for automotive parts, household products, and pharmaceutical and food packaging. Voridian PET thermoplastic polyesters are condensation polymers produced by a continuous melt-phase polymerization process followed by a solid-state polymerization process. It is a copolymer PET that has been crystallized. Color concentrates, additives, and denest versions of 9921 are available on request.

Applications/Uses

  • APET sheet
  • Automotive parts containers
  • Food packaging
  • Household products containers
  • Pharmaceutical containers
  • Wine and liquor containers
  • Water bottles
  • Carbonated soft drink bottles
  • Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Bulk Density 0.817 g/cc0.0295 lb/in³Poured; ASTM D1895
     0.881 g/cc0.0318 lb/in³Vibrated; ASTM D1895
    Density 1.33 g/cc0.0480 lb/in³Film; ASTM D1505
     1.40 g/cc0.0506 lb/in³Crystalline Density; ASTM D1505
    Melt Density 1.20 g/cc
    @Temperature 285 °C
    0.0434 lb/in³
    @Temperature 545 °F
    ASTM D1238
    Particle Size 2500 µm2500 µmPellet Size
    Water Vapor Transmission 6.00 g/m²/day0.386 g/100 in²/dayASTM F372
    Oxygen Transmission 5.10 cc-mm/m²-24hr-atm13.0 cc-mil/100 in²-24hr-atmASTM D3985
    Carbon Dioxide Transmission 28.0 cc-mm/m²-24hr-atm71.1 cc-mil/100 in²-24hr-atmASTM D1434
    Viscosity Measurement 0.750.75Intrinsic; EMN-A-AC-G-V-1
     0.78 - 0.820.78 - 0.82Pellet, Intrinsic; VGAS-A-AN-G-V-1
    Thickness 250 microns9.84 mil
     
    Mechanical PropertiesMetricEnglishComments
    Film Tensile Strength at Yield, MD 59.0 MPa8560 psiASTM D882
    Film Tensile Strength at Yield, TD 57.0 MPa8270 psiASTM D882
    Film Elongation at Break, MD 300 %300 %ASTM D882
    Film Elongation at Break, TD 200 %200 %ASTM D882
    Film Elongation at Yield, MD 4.0 %4.0 %ASTM D882
    Film Elongation at Yield, TD 4.0 %4.0 %ASTM D882
    Tensile Modulus 2.20 GPa319 ksiTD; ASTM D882
     2.20 GPa319 ksiMD; ASTM D882
    Izod Impact, Unnotched (ISO) NBNBISO 180
     160 kJ/m²
    @Temperature -40.0 °C
    76.1 ft-lb/in²
    @Temperature -40.0 °F
    ISO 180
    Tear Strength, Total 15.0 N3.37 lb (f)Split Tear Method, 254mm/min, MD; ASTM D1938
     16.0 N3.60 lb (f)Split Tear Method, 254mm/min, TD; ASTM D1938
     102 N22.9 lb (f)PPT Tear Resistance, MD; ASTM D2582
     120 N27.0 lb (f)PPT Tear Resistance, TD; ASTM D2582
    Tear Strength 54.0 kN/m308 pliTrouser Tear Resistance, MD; ISO 6383-1
     59.0 kN/m337 pliTrouser Tear Resistance, TD; ISO 6383-1
    Elmendorf Tear Strength, MD 4.00 g/micron102 g/milASTM D1922
    Elmendorf Tear Strength, TD 5.20 g/micron132 g/milASTM D1922
    Dart Drop 1.60 g/micron40.6 g/milat -18°C; ASTM D1709
     2.00 g/micron50.8 g/mil23°C; ASTM D1709
    Film Tensile Strength at Break, MD 58.0 MPa8410 psiASTM D882
    Film Tensile Strength at Break, TD 39.0 MPa5660 psiASTM D882
     
    Thermal PropertiesMetricEnglishComments
    Heat of Fusion 56.0 J/g24.1 BTU/lbASTM E793
    Specific Heat Capacity 1.10 J/g-°C0.263 BTU/lb-°FASTM E1269
     1.30 J/g-°C
    @Temperature 80.0 °C
    0.311 BTU/lb-°F
    @Temperature 176 °F
    ASTM E1269
     1.40 J/g-°C
    @Temperature 100 °C
    0.335 BTU/lb-°F
    @Temperature 212 °F
    ASTM E1269
     1.90 J/g-°C
    @Temperature 200 °C
    0.454 BTU/lb-°F
    @Temperature 392 °F
    ASTM E1269
     2.10 J/g-°C
    @Temperature 280 °C
    0.502 BTU/lb-°F
    @Temperature 536 °F
    ASTM E1269
    Melting Point 245 °C473 °FCrystalline Peak; ASTM D3418
     
    Optical PropertiesMetricEnglishComments
    Haze 0.80 %0.80 %ASTM D1003
    Gloss 108 %108 %at 45°; ASTM D2457
    Transmission, Visible 85 %85 %Transparency; ASTM D1746
     89 %89 %Regular Transmittance; ASTM D1003
     91 %91 %Total Transmittance; ASTM D1003
     
    Descriptive Properties
    Acetaldehyde<1ppmVKCA-A-AS-G-GC-0001
    Color, CIE a*-3.8 to -0.8VGAS-A-AN-G-RS-001
    Color, CIE b*-2.3 to 1.7VGAS-A-AN-G-RS-001
    Color, CIE L*78 minVGAS-A-AN-G-RS-001
    Fines, wt%, max0.05VGAS-A-AN-G-GA-1
    Pellet ShapeCubical

    **
    Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

    Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Eastman 9921 PET Film
    Eastman 9921P PET Film
    Chengdu Polyster PET Film PET Films/Sheets
    DuPont Teijin Films Melinex® HC-1 Planarised PET film
    Solvay P720X PET-Based Release Film

    PE9138 / 35195

    Aluminum Castings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.