MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

AISI 1015 Steel, cold drawn
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: The composition listed is only for structural shapes, plate, sheet, strip, and welded tubing. Hot-rolled and cold finished bars, semifinished products for forging, wire rods, and seamless tubing have a carbon content of 0.13 - 0.18%. Has better machinability and carburizing characteristics than the more formable extra-low carbon steels.

Applications: cold-formed, cold-headed, or forged parts which are low strength with hard, wear resistant surfaces.

Key Words: UNS G10150, AISI1015
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.87 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 111111
Hardness, Knoop 129129
Hardness, Rockwell B 6464Converted from Brinell
Hardness, Vickers 115115Converted from Brinell
Tensile Strength, Ultimate 385 MPa55800 psi
Tensile Strength, Yield 325 MPa47100 psi
Elongation at Break 18 %18 %In 50 mm
Reduction of Area 40 %40 %
Modulus of Elasticity 205 GPa29700 ksiTypical for steel
Bulk Modulus 160 GPa23200 ksiTypical for steel
Poissons Ratio 0.290.29Typical For Steel
Machinability 60 %60 %Based on 100% machinability for AISI 1212 steel.
Shear Modulus 80.0 GPa11600 ksiTypical for steel
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000159 ohm-cm
@Temperature 0.000 °C
0.0000159 ohm-cm
@Temperature 32.0 °F
annealed condition
 0.0000219 ohm-cm
@Temperature 100 °C
0.0000219 ohm-cm
@Temperature 212 °F
annealed condition
 0.0000292 ohm-cm
@Temperature 200 °C
0.0000292 ohm-cm
@Temperature 392 °F
annealed condition
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.9 µm/m-°C
@Temperature 0.000 - 100 °C
6.61 µin/in-°F
@Temperature 32.0 - 212 °F
 13.0 µm/m-°C
@Temperature 0.000 - 300 °C
7.22 µin/in-°F
@Temperature 32.0 - 572 °F
 14.2 µm/m-°C
@Temperature 0.000 - 500 °C
7.89 µin/in-°F
@Temperature 32.0 - 932 °F
Specific Heat Capacity 0.486 J/g-°C
@Temperature >=100 °C
0.116 BTU/lb-°F
@Temperature >=212 °F
annealed
Thermal Conductivity 51.9 W/m-K360 BTU-in/hr-ft²-°Festimated based on similar materials
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.13 - 0.18 %0.13 - 0.18 %
Iron, Fe 99.13 - 99.57 %99.13 - 99.57 %As remainder
Manganese, Mn 0.30 - 0.60 %0.30 - 0.60 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S <= 0.050 %<= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1010 Steel, cold drawn
AISI 1018 Steel, cold drawn
AISI 1015 Steel, as rolled
AISI 1012 Steel, cold drawn
AISI 1020 Steel, cold rolled

M1015A / 6790

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.