MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Lubrizol ESTANE® 58134 Ester Based Thermoplastic Polyurethane
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Features: Fast cycling, broad temperature performance, and durability

Uses: Injection Molding

Available in Americas, Europe, Middle East, Africa, India and Asia

Information provided by Lubrizol.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.22 g/cc1.22 g/ccASTM D792
Maximum Moisture Content 0.0200.020
Linear Mold Shrinkage 0.0090 cm/cm0.0090 in/inflex bar, Injection
 0.013 cm/cm0.013 in/indisk, Injection
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 42 - 48
@Time 5.00 sec
42 - 48
@Time 0.00139 hour
ASTM D2240
Tensile Strength 40.0 MPa5800 psiASTM D412
Elongation at Break 500 %500 %ASTM D412
100% Modulus 9.00 MPa
@Strain 100 %
1310 psi
@Strain 100 %
ASTM D412
300% Modulus 20.0 MPa
@Strain 300 %
2900 psi
@Strain 300 %
ASTM D412
Flexural Modulus 0.0593 GPa8.60 ksiASTM D790
Tear Strength 36.8 kN/m210 pliTrouser; ASTM D470
Graves Tear Strength 128 kN/m730 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 6262CS-17, 1000 g; ASTM D3389 B
Compression Set  35 %
@Temperature 23.0 °C,
Time 79200 sec
35 %
@Temperature 73.4 °F,
Time 22.0 hour
ASTM D395
 39 %
@Temperature 70.0 °C,
Time 79200 sec
39 %
@Temperature 158 °F,
Time 22.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
Melting Point 216 °C421 °FDSC
Glass Transition Temp, Tg -46.0 °C-50.8 °FDSC
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 204 °C399 °FInjection
Middle Barrel Temperature 210 °C410 °FInjection
Front Barrel Temperature 218 °C424 °FInjection
Nozzle Temperature 221 °C430 °FInjection
Melt Temperature 221 °C430 °FInjection
Drying Temperature 104 °C219 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Dew Point -40.0 °C-40.0 °F
Injection Pressure 10000 - 15000 MPa1.45e+6 - 2.18e+6 psiInjection
Hold Pressure 5000 - 10000 MPa725000 - 1.45e+6 psiInjection
Back Pressure >= 50.0 MPa>= 7250 psiInjection
Screw Speed 60 - 100 rpm60 - 100 rpmInjection

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Lubrizol Advanced Materials PEARLTHANE® 11T93 Thermoplastic Polyurethane Elastomer
Lubrizol ESTANE® 58130 Ester Based Thermoplastic Polyurethane
DuPont Mobility and Materials Delrin® 500P NC010 POM
Lubrizol ESTANE® 58215 Ether Based Thermoplastic Polyurethane
Metflex EM67 Natural Rubber

PNOVEON024 / 55290

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.