System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Menzolit Menzolit® BMC 0160 Unsaturated Polyester UP
Categories:
Polymer
;
Thermoset
;
Polyester, TS
;
Thermoset Polyester Glass Filled BMC
Material Notes:
BMC 0160 is a general purpose BMC for electrical applications. Typical applications are lamp housings, canopies, covers and similar components.
Information Provided by Menzolit
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
1.90
g/cc
0.0686
lb/in³
ISO 1183
Water Absorption
<= 0.50 %
<= 0.50 %
ISO 62
Linear Mold Shrinkage
0.0015
cm/cm
0.0015
in/in
ISO 2577
Mechanical Properties
Metric
English
Comments
Tensile Strength, Ultimate
31.0
MPa
@Temperature 22.0 °C
4500
psi
@Temperature 71.6 °F
25 mm flat samples, compression molded; ISO 527-4
Tensile Strength, Yield
31.0
MPa
@Temperature 22.0 °C
4500
psi
@Temperature 71.6 °F
25 mm flat samples, compression molded; ISO 527-4
Elongation at Break
0.00 %
0.00 %
ISO 527-4
Modulus of Elasticity
13.0
GPa
1890
ksi
25 mm flat samples, compression molded; ISO 527-4
Flexural Strength
100
MPa
@Temperature 22.0 °C
14500
psi
@Temperature 71.6 °F
25 mm wide 100 mm long, flat samples; ISO 14125
Flexural Modulus
10.0
GPa
@Temperature 22.0 °C
1450
ksi
@Temperature 71.6 °F
25 mm wide 100 mm long, flat samples; ISO 14125
Poissons Ratio
0.30
0.30
Shear Modulus
5.00
GPa
725
ksi
in plane
Charpy Impact, Notched
3.00
J/cm²
14.3
ft-lb/in²
ISO 179
Electrical Properties
Metric
English
Comments
Volume Resistivity
1.00e+15
ohm-cm
1.00e+15
ohm-cm
IEC 60093
Surface Resistance
1.00e+12
ohm
1.00e+12
ohm
IEC 60093
Dielectric Constant
4.0
4.0
IEC 60250
Dielectric Strength
30.0
kV/mm
762
kV/in
IEC 60243-1
Dissipation Factor
0.010
0.010
IEC 60250
Comparative Tracking Index
600
V
600
V
IEC 60112
Thermal Properties
Metric
English
Comments
CTE, linear
10.0
µm/m-°C
5.56
µin/in-°F
ISO 11359-2
Specific Heat Capacity
1.10
J/g-°C
0.263
BTU/lb-°F
Thermal Conductivity
0.700
W/m-K
4.86
BTU-in/hr-ft²-°F
Maximum Service Temperature, Air
165
°C
329
°F
Deflection Temperature at 1.8 MPa (264 psi)
>=
130
°C
>=
266
°F
ISO 75-2
Minimum Service Temperature, Air
-40.0
°C
-40.0
°F
Glass Transition Temp, Tg
170
°C
338
°F
ISO 11357-2
Flammability, UL94
V-0
@Thickness 3.00 mm
V-0
@Thickness 0.118 in
Oxygen Index
30 %
30 %
ISO 4589-2
Glow Wire Flammability Index
750
°C
1380
°F
IEC 60695-2-12
Processing Properties
Metric
English
Comments
Processing Temperature
135
-
155
°C
275
-
311
°F
Injection molding, matched metal die
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Menzolit Menzolit® BMC 0180 Unsaturated Polyester UP
Menzolit Menzolit® BMC 0170 Unsaturated Polyester UP
Bakelite® UP 802 Unsaturated Polyester Resin, High Surface Quality, Low Shrinkage, High Arc Resistance
Bakelite® UP 3415 Unsaturated Polyester Resin, Low Shrinkage, High Arc Resistance, UL Listed, High Mechanical Strength
C.O.I.M. FILCO® 656 Unsaturated Polyester Powder Resin
PMENZ001 / 100735
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.