MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Solvay VTA® 260 Adhesive Film
Categories: Polymer; Adhesive; Film

Material Notes: Description: VTA®260 is a variable cure temperature film adhesive suitable for bonding both composite substrates and aluminum to themselves or to honeycomb and foam core materials. VTA260 is fully cure compatible with Cytec’s VTM pregreg range.

Features & Benefits:

  • 30 days out life at 21°C (70°F)
  • 12 months storage at -18°C (0°F)
  • Flexible cure between 65 and 120°C (149 and 248°F)
  • Minimum cure temperature 65°C (149°F)
  • Good tack for easy lay-up of large structures, vertical surfaces and complex shapes
  • Maximum dry service temperature of 120°C (248°F) after full post-cure

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³Cured Resin
Storage Temperature -18.0 °C-0.400 °F
 
Mechanical PropertiesMetricEnglishComments
Shear Strength  6.00 MPa
@Temperature 80.0 °C
870 psi
@Temperature 176 °F
Lap, 16 hrs at 65°C, Material: PK13-313g/m3; ASTM D3165-00
 15.0 MPa
@Temperature 120 °C
2180 psi
@Temperature 248 °F
Lap, 1 hr at 120°C, Material: PK13-313g/m3; ASTM D3165-00
 16.0 MPa
@Temperature 80.0 °C
2320 psi
@Temperature 176 °F
Lap, 5 hrs at 80°C, Material: PK13-313g/m3; ASTM D3165-00
 23.0 MPa
@Temperature 21.0 °C
3340 psi
@Temperature 69.8 °F
Lap, 16 hrs at 65°C, Material: PK13-313g/m3; ASTM D3165-00
 26.0 MPa
@Temperature 80.0 °C
3770 psi
@Temperature 176 °F
Lap, 1 hr at 120°C, Material: PK13-313g/m3; ASTM D3165-00
 30.0 MPa
@Temperature 21.0 °C
4350 psi
@Temperature 69.8 °F
Lap, 5 hrs at 80°C, Material: PK13-313g/m3; ASTM D3165-00
 38.0 MPa
@Temperature 21.0 °C
5510 psi
@Temperature 69.8 °F
Lap, 1 hr at 120°C, Material: PK13-313g/m3; ASTM D3165-00
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 80.0 °C176 °Ffor cure 5 hrs at 80°C
 110 °C230 °Ffor cure 2 hrs at 100°C
 120 °C248 °Ffor cure 1 hrs at 120°C
 
Processing PropertiesMetricEnglishComments
Cure Time  60.0 min
@Temperature 120 °C
1.00 hour
@Temperature 248 °F
 120 min
@Temperature 100 °C
2.00 hour
@Temperature 212 °F
 300 min
@Temperature 80.0 °C
5.00 hour
@Temperature 176 °F
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
ColorPink

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elantas Conap FR-1046 / EA-02 Conapoxy® Resin / Conacure® Hardener
Solvay FM® 377S Adhesive Film, psf 0.06 (293 gsm)
Solvay VTF 261 Film
Solvay Thornel® T-605/50X 12K Carbon Fiber, Polyacrylonitrile (PAN) Precursor
Solvay Thornel® T-40 12K Carbon Fiber, Polyacrylonitrile (PAN) Precursor

PCYTED109 / 180411

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.