MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

DuPont Mobility and Materials Zytel® RS LC1000 BK385 Nylon 1010 (With Extended Stress-Strain Tabular Data)  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: UV Stabilized Renewably Sourced Polyamide 1010 Developed for Extrusion

Zytel RS LC1000 BK385 is a renewable sourced Polyamide 1010 containing a minimum of 90% renewably sourced ingredient by weight. The material is flexible unreinforced UV and heat sta

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Key Words: PA1010
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³DAM; ISO 1183
Moisture Absorption 1.00 %
@Thickness 2.00 mm
1.00 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Viscosity Test 130 cm³/g1.30 dl/gISO 307 1157 1628
Linear Mold Shrinkage, Flow 0.014 cm/cm0.014 in/inDAM; ISO 294-4 2577
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inDAM; ISO 294-4 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 49.0 MPa7110 psi50%RH; ISO 527-1/-2
 60.0 MPa8700 psiDAM; ISO 527-1/-2
Tensile Stress at Strain  0.270 MPa
@Strain 0.07 %,
Temperature 150 °C
39.2 psi
@Strain 0.07 %,
Temperature 302 °F
50%RH; ISO 11403-1 -2
 0.300 MPa
@Strain 0.08 %,
Temperature 150 °C
43.5 psi
@Strain 0.08 %,
Temperature 302 °F
DAM; ISO 11403-1 -2
 0.450 MPa
@Strain 0.03 %,
Temperature -40.0 °C
65.3 psi
@Strain 0.03 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 0.450 MPa
@Strain 0.1 %,
Temperature 90.0 °C
65.3 psi
@Strain 0.1 %,
Temperature 194 °F
50%RH; ISO 11403-1 -2
 0.480 MPa
@Strain 0.02 %,
Temperature -40.0 °C
69.6 psi
@Strain 0.02 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 0.490 MPa
@Strain 0.09 %,
Temperature 90.0 °C
71.1 psi
@Strain 0.09 %,
Temperature 194 °F
DAM; ISO 11403-1 -2
 0.750 MPa
@Strain 0.04 %,
Temperature -20.0 °C
109 psi
@Strain 0.04 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 0.840 MPa
@Strain 0.08 %,
Temperature 40.0 °C
122 psi
@Strain 0.08 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 0.840 MPa
@Strain 0.05 %,
Temperature -20.0 °C
122 psi
@Strain 0.05 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 0.930 MPa
@Strain 0.02 %,
Temperature 0.000 °C
135 psi
@Strain 0.02 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 1.03 MPa
@Strain 0.07 %,
Temperature 40.0 °C
149 psi
@Strain 0.07 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 1.29 MPa
@Strain 0.06 %,
Temperature 23.0 °C
187 psi
@Strain 0.06 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 1.39 MPa
@Strain 0.05 %,
Temperature 0.000 °C
202 psi
@Strain 0.05 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 1.70 MPa
@Strain 0.06 %,
Temperature 23.0 °C
247 psi
@Strain 0.06 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 1.78 MPa
@Strain 0.1 %,
Temperature -40.0 °C
258 psi
@Strain 0.1 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 1.92 MPa
@Strain 0.11 %,
Temperature -40.0 °C
278 psi
@Strain 0.11 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 2.85 MPa
@Strain 0.11 %,
Temperature 0.000 °C
413 psi
@Strain 0.11 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 3.15 MPa
@Strain 0.17 %,
Temperature -20.0 °C
457 psi
@Strain 0.17 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 3.37 MPa
@Strain 0.14 %,
Temperature -20.0 °C
489 psi
@Strain 0.14 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 3.69 MPa
@Strain 0.18 %,
Temperature -40.0 °C
535 psi
@Strain 0.18 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 3.72 MPa
@Strain 0.18 %,
Temperature -40.0 °C
540 psi
@Strain 0.18 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 4.22 MPa
@Strain 0.25 %,
Temperature 23.0 °C
612 psi
@Strain 0.25 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 4.37 MPa
@Strain 0.18 %,
Temperature 0.000 °C
634 psi
@Strain 0.18 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 4.71 MPa
@Strain 0.19 %,
Temperature 0.000 °C
683 psi
@Strain 0.19 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 4.78 MPa
@Strain 2.86 %,
Temperature 150 °C
693 psi
@Strain 2.86 %,
Temperature 302 °F
50%RH; ISO 11403-1 -2
 5.09 MPa
@Strain 0.23 %,
Temperature 23.0 °C
738 psi
@Strain 0.23 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 5.35 MPa
@Strain 0.25 %,
Temperature -40.0 °C
776 psi
@Strain 0.25 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 5.45 MPa
@Strain 0.25 %,
Temperature -40.0 °C
790 psi
@Strain 0.25 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 5.74 MPa
@Strain 0.23 %,
Temperature -20.0 °C
833 psi
@Strain 0.23 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 5.84 MPa
@Strain 3.2 %,
Temperature 150 °C
847 psi
@Strain 3.2 %,
Temperature 302 °F
DAM; ISO 11403-1 -2
 6.48 MPa
@Strain 0.43 %,
Temperature 40.0 °C
940 psi
@Strain 0.43 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 10.0 MPa
@Strain 13.37 %,
Temperature 150 °C
1450 psi
@Strain 13.37 %,
Temperature 302 °F
50%RH; ISO 11403-1 -2
 11.04 MPa
@Strain 2.94 %,
Temperature 90.0 °C
1601 psi
@Strain 2.94 %,
Temperature 194 °F
DAM; ISO 11403-1 -2
 11.12 MPa
@Strain 14 %,
Temperature 150 °C
1613 psi
@Strain 14 %,
Temperature 302 °F
DAM; ISO 11403-1 -2
 11.26 MPa
@Strain 24.48 %,
Temperature 150 °C
1633 psi
@Strain 24.48 %,
Temperature 302 °F
50%RH; ISO 11403-1 -2
 11.43 MPa
@Strain 70.4 %,
Temperature 150 °C
1658 psi
@Strain 70.4 %,
Temperature 302 °F
50%RH; ISO 11403-1 -2
 11.6 MPa
@Strain 100.03 %,
Temperature 150 °C
1680 psi
@Strain 100.03 %,
Temperature 302 °F
50%RH; ISO 11403-1 -2
 12.25 MPa
@Strain 25.96 %,
Temperature 150 °C
1777 psi
@Strain 25.96 %,
Temperature 302 °F
DAM; ISO 11403-1 -2
 12.31 MPa
@Strain 71.22 %,
Temperature 150 °C
1785 psi
@Strain 71.22 %,
Temperature 302 °F
DAM; ISO 11403-1 -2
 12.48 MPa
@Strain 100.05 %,
Temperature 150 °C
1810 psi
@Strain 100.05 %,
Temperature 302 °F
DAM; ISO 11403-1 -2
 12.64 MPa
@Strain 4.33 %,
Temperature 90.0 °C
1833 psi
@Strain 4.33 %,
Temperature 194 °F
50%RH; ISO 11403-1 -2
 19.82 MPa
@Strain 14.51 %,
Temperature 90.0 °C
2875 psi
@Strain 14.51 %,
Temperature 194 °F
50%RH; ISO 11403-1 -2
 19.95 MPa
@Strain 2.38 %,
Temperature 40.0 °C
2894 psi
@Strain 2.38 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 21.17 MPa
@Strain 73.09 %,
Temperature 90.0 °C
3070 psi
@Strain 73.09 %,
Temperature 194 °F
50%RH; ISO 11403-1 -2
 21.22 MPa
@Strain 26.5 %,
Temperature 90.0 °C
3078 psi
@Strain 26.5 %,
Temperature 194 °F
50%RH; ISO 11403-1 -2
 21.41 MPa
@Strain 13.33 %,
Temperature 90.0 °C
3105 psi
@Strain 13.33 %,
Temperature 194 °F
DAM; ISO 11403-1 -2
 21.59 MPa
@Strain 100.03 %,
Temperature 90.0 °C
3131 psi
@Strain 100.03 %,
Temperature 194 °F
50%RH; ISO 11403-1 -2
 22.9 MPa
@Strain 72.74 %,
Temperature 90.0 °C
3320 psi
@Strain 72.74 %,
Temperature 194 °F
DAM; ISO 11403-1 -2
 22.97 MPa
@Strain 25.83 %,
Temperature 90.0 °C
3332 psi
@Strain 25.83 %,
Temperature 194 °F
DAM; ISO 11403-1 -2
 23.42 MPa
@Strain 100.03 %,
Temperature 90.0 °C
3397 psi
@Strain 100.03 %,
Temperature 194 °F
DAM; ISO 11403-1 -2
 24.01 MPa
@Strain 1.04 %,
Temperature -20.0 °C
3482 psi
@Strain 1.04 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 30.88 MPa
@Strain 1.41 %,
Temperature 0.000 °C
4479 psi
@Strain 1.41 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 34.21 MPa
@Strain 70.99 %,
Temperature 40.0 °C
4962 psi
@Strain 70.99 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 34.57 MPa
@Strain 100.03 %,
Temperature 40.0 °C
5014 psi
@Strain 100.03 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 36.0 MPa
@Strain 12.5 %,
Temperature 40.0 °C
5220 psi
@Strain 12.5 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 37.15 MPa
@Strain 24.59 %,
Temperature 40.0 °C
5388 psi
@Strain 24.59 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 38.31 MPa
@Strain 68.85 %,
Temperature 40.0 °C
5556 psi
@Strain 68.85 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 39.49 MPa
@Strain 100.05 %,
Temperature 40.0 °C
5728 psi
@Strain 100.05 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 39.52 MPa
@Strain 70.06 %,
Temperature 23.0 °C
5732 psi
@Strain 70.06 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 39.63 MPa
@Strain 100.04 %,
Temperature 23.0 °C
5748 psi
@Strain 100.04 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 40.84 MPa
@Strain 9.98 %,
Temperature 40.0 °C
5923 psi
@Strain 9.98 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 42.52 MPa
@Strain 21.74 %,
Temperature 40.0 °C
6167 psi
@Strain 21.74 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 42.81 MPa
@Strain 71.61 %,
Temperature 23.0 °C
6209 psi
@Strain 71.61 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 43.39 MPa
@Strain 100.04 %,
Temperature 23.0 °C
6293 psi
@Strain 100.04 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 48.1 MPa
@Strain 54.79 %,
Temperature 0.000 °C
6980 psi
@Strain 54.79 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 48.9 MPa
@Strain 79.54 %,
Temperature 0.000 °C
7090 psi
@Strain 79.54 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 49.05 MPa
@Strain 8.61 %,
Temperature 23.0 °C
7114 psi
@Strain 8.61 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 49.85 MPa
@Strain 22.96 %,
Temperature 0.000 °C
7230 psi
@Strain 22.96 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 50.27 MPa
@Strain 38.36 %,
Temperature 0.000 °C
7291 psi
@Strain 38.36 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 50.29 MPa
@Strain 19.74 %,
Temperature 23.0 °C
7294 psi
@Strain 19.74 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 50.47 MPa
@Strain 2.35 %,
Temperature -20.0 °C
7320 psi
@Strain 2.35 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 51.63 MPa
@Strain 43.68 %,
Temperature -20.0 °C
7488 psi
@Strain 43.68 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 52.02 MPa
@Strain 2.65 %,
Temperature 0.000 °C
7545 psi
@Strain 2.65 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 53.44 MPa
@Strain 19.88 %,
Temperature 23.0 °C
7751 psi
@Strain 19.88 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 54.0 MPa
@Strain 27.41 %,
Temperature -20.0 °C
7830 psi
@Strain 27.41 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 54.49 MPa
@Strain 20.94 %,
Temperature -20.0 °C
7903 psi
@Strain 20.94 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 55.41 MPa
@Strain 34.32 %,
Temperature -20.0 °C
8037 psi
@Strain 34.32 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 59.12 MPa
@Strain 6.81 %,
Temperature 23.0 °C
8575 psi
@Strain 6.81 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 66.43 MPa
@Strain 11.77 %,
Temperature 0.000 °C
9635 psi
@Strain 11.77 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 71.91 MPa
@Strain 4.65 %,
Temperature -20.0 °C
10430 psi
@Strain 4.65 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 84.01 MPa
@Strain 18.92 %,
Temperature -40.0 °C
12180 psi
@Strain 18.92 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 89.32 MPa
@Strain 9.59 %,
Temperature -40.0 °C
12950 psi
@Strain 9.59 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 91.05 MPa
@Strain 13.49 %,
Temperature -40.0 °C
13210 psi
@Strain 13.49 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 94.14 MPa
@Strain 7.53 %,
Temperature -40.0 °C
13650 psi
@Strain 7.53 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
Elongation at Break 50 %50 %DAM; Nominal; ISO 527-1/-2
 >= 50 %>= 50 %50%RH; Nominal; ISO 527-1/-2
Elongation at Yield 4.6 %4.6 %DAM; ISO 527-1/-2
 24 %24 %50%RH; ISO 527-1/-2
Tensile Modulus 1.16 GPa168 ksi50%RH; ISO 527-1/-2
 2.10 GPa305 ksiDAM; ISO 527-1/-2
 0.295 GPa
@Temperature 120 °C
42.8 ksi
@Temperature 248 °F
50%RH; ISO 11403-1 -2
 0.311 GPa
@Temperature 120 °C
45.1 ksi
@Temperature 248 °F
DAM; ISO 11403-1 -2
 0.886 GPa
@Temperature 40.0 °C
129 ksi
@Temperature 104 °F
50%RH; ISO 11403-1 -2
 1.249 GPa
@Temperature 40.0 °C
181.2 ksi
@Temperature 104 °F
DAM; ISO 11403-1 -2
 2.388 GPa
@Temperature -40.0 °C
346.4 ksi
@Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 2.407 GPa
@Temperature -40.0 °C
349.1 ksi
@Temperature -40.0 °F
DAM; ISO 11403-1 -2
Flexural Modulus 1.74 GPa252 ksiDAM; ISO 178
Secant Modulus  0.0445 GPa
@Strain 76.78 %,
Temperature 40.0 °C
6.45 ksi
@Strain 76.78 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 0.0509 GPa
@Strain 75.16 %,
Temperature 40.0 °C
7.39 ksi
@Strain 75.16 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 0.051979 GPa
@Strain 76.05 %,
Temperature 23.0 °C
7.5390 ksi
@Strain 76.05 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 0.0555 GPa
@Strain 77.29 %,
Temperature 23.0 °C
8.05 ksi
@Strain 77.29 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 0.0644 GPa
@Strain 54.17 %,
Temperature 40.0 °C
9.34 ksi
@Strain 54.17 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 0.0755 GPa
@Strain 52.11 %,
Temperature 23.0 °C
10.9 ksi
@Strain 52.11 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 0.0783 GPa
@Strain 54.53 %,
Temperature 23.0 °C
11.4 ksi
@Strain 54.53 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 0.079326 GPa
@Strain 50.74 %,
Temperature 40.0 °C
11.505 ksi
@Strain 50.74 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 0.0809 GPa
@Strain 59.71 %,
Temperature 0.000 °C
11.7 ksi
@Strain 59.71 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 0.108 GPa
@Strain 33.72 %,
Temperature 40.0 °C
15.7 ksi
@Strain 33.72 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 0.119 GPa
@Strain 40.08 %,
Temperature 0.000 °C
17.3 ksi
@Strain 40.08 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 0.13477 GPa
@Strain 31.78 %,
Temperature 23.0 °C
19.547 ksi
@Strain 31.78 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 0.138 GPa
@Strain 30.48 %,
Temperature 40.0 °C
20.0 ksi
@Strain 30.48 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 0.165 GPa
@Strain 30.98 %,
Temperature -20.0 °C
23.9 ksi
@Strain 30.98 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 0.172 GPa
@Strain 28.46 %,
Temperature 23.0 °C
24.9 ksi
@Strain 28.46 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 0.195 GPa
@Strain 25.9 %,
Temperature 0.000 °C
28.2 ksi
@Strain 25.9 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 0.226 GPa
@Strain 16.33 %,
Temperature 40.0 °C
32.8 ksi
@Strain 16.33 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 0.233 GPa
@Strain 23.53 %,
Temperature -20.0 °C
33.8 ksi
@Strain 23.53 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 0.305 GPa
@Strain 13.76 %,
Temperature 40.0 °C
44.2 ksi
@Strain 13.76 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 0.329 GPa
@Strain 19.64 %,
Temperature 0.000 °C
47.7 ksi
@Strain 19.64 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 0.412 GPa
@Strain 12.15 %,
Temperature 23.0 °C
59.8 ksi
@Strain 12.15 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 0.433 GPa
@Strain 17.17 %,
Temperature -20.0 °C
62.9 ksi
@Strain 17.17 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 0.518 GPa
@Strain 10.94 %,
Temperature 23.0 °C
75.1 ksi
@Strain 10.94 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 0.538 GPa
@Strain 12.72 %,
Temperature 0.000 °C
78.0 ksi
@Strain 12.72 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 0.691 GPa
@Strain 11.35 %,
Temperature -20.0 °C
100 ksi
@Strain 11.35 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 0.791 GPa
@Strain 11.24 %,
Temperature -40.0 °C
115 ksi
@Strain 11.24 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 0.838 GPa
@Strain 2.38 %,
Temperature 40.0 °C
122 ksi
@Strain 2.38 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 0.945 GPa
@Strain 8.15 %,
Temperature -20.0 °C
137 ksi
@Strain 8.15 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 1.05 GPa
@Strain 0.08 %,
Temperature 40.0 °C
152 ksi
@Strain 0.08 %,
Temperature 104 °F
50%RH; ISO 11403-1 -2
 1.09 GPa
@Strain 8.72 %,
Temperature -40.0 °C
158 ksi
@Strain 8.72 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 1.29 GPa
@Strain 5.1 %,
Temperature 0.000 °C
187 ksi
@Strain 5.1 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 1.47 GPa
@Strain 0.07 %,
Temperature 40.0 °C
213 ksi
@Strain 0.07 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 1.50 GPa
@Strain 0.03 %,
Temperature -40.0 °C
218 ksi
@Strain 0.03 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 1.51 GPa
@Strain 0.43 %,
Temperature 40.0 °C
219 ksi
@Strain 0.43 %,
Temperature 104 °F
DAM; ISO 11403-1 -2
 1.53 GPa
@Strain 5.48 %,
Temperature -40.0 °C
222 ksi
@Strain 5.48 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 1.68 GPa
@Strain 0.05 %,
Temperature -20.0 °C
244 ksi
@Strain 0.05 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 1.688 GPa
@Strain 0.25 %,
Temperature 23.0 °C
244.8 ksi
@Strain 0.25 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 1.72 GPa
@Strain 4.47 %,
Temperature -20.0 °C
249 ksi
@Strain 4.47 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 1.75 GPa
@Strain 0.11 %,
Temperature -40.0 °C
253 ksi
@Strain 0.11 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 1.76 GPa
@Strain 4.64 %,
Temperature -40.0 °C
255 ksi
@Strain 4.64 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 1.77 GPa
@Strain 3.76 %,
Temperature 0.000 °C
257 ksi
@Strain 3.76 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 1.78 GPa
@Strain 0.1 %,
Temperature -40.0 °C
258 ksi
@Strain 0.1 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 1.85 GPa
@Strain 0.17 %,
Temperature -20.0 °C
269 ksi
@Strain 0.17 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 1.875 GPa
@Strain 0.04 %,
Temperature -20.0 °C
271.9 ksi
@Strain 0.04 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 2.13 GPa
@Strain 0.2 %,
Temperature -40.0 °C
309 ksi
@Strain 0.2 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 2.14 GPa
@Strain 0.2 %,
Temperature -40.0 °C
310 ksi
@Strain 0.2 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 2.15 GPa
@Strain 0.06 %,
Temperature 23.0 °C
312 ksi
@Strain 0.06 %,
Temperature 73.4 °F
50%RH; ISO 11403-1 -2
 2.15 GPa
@Strain 2.18 %,
Temperature -20.0 °C
312 ksi
@Strain 2.18 %,
Temperature -4.00 °F
50%RH; ISO 11403-1 -2
 2.21 GPa
@Strain 0.23 %,
Temperature 23.0 °C
321 ksi
@Strain 0.23 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 2.22 GPa
@Strain 1.68 %,
Temperature -40.0 °C
322 ksi
@Strain 1.68 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 2.28 GPa
@Strain 1.93 %,
Temperature -40.0 °C
331 ksi
@Strain 1.93 %,
Temperature -40.0 °F
50%RH; ISO 11403-1 -2
 2.30 GPa
@Strain 0.23 %,
Temperature 0.000 °C
334 ksi
@Strain 0.23 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 2.40 GPa
@Strain 0.02 %,
Temperature -40.0 °C
348 ksi
@Strain 0.02 %,
Temperature -40.0 °F
DAM; ISO 11403-1 -2
 2.41 GPa
@Strain 0.14 %,
Temperature -20.0 °C
349 ksi
@Strain 0.14 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 2.43 GPa
@Strain 0.18 %,
Temperature 0.000 °C
352 ksi
@Strain 0.18 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 2.428 GPa
@Strain 0.5 %,
Temperature -20.0 °C
352.2 ksi
@Strain 0.5 %,
Temperature -4.00 °F
DAM; ISO 11403-1 -2
 2.59 GPa
@Strain 0.11 %,
Temperature 0.000 °C
376 ksi
@Strain 0.11 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
 2.78 GPa
@Strain 0.05 %,
Temperature 0.000 °C
403 ksi
@Strain 0.05 %,
Temperature 32.0 °F
50%RH; ISO 11403-1 -2
 2.83 GPa
@Strain 0.06 %,
Temperature 23.0 °C
411 ksi
@Strain 0.06 %,
Temperature 73.4 °F
DAM; ISO 11403-1 -2
 4.65 GPa
@Strain 0.02 %,
Temperature 0.000 °C
674 ksi
@Strain 0.02 %,
Temperature 32.0 °F
DAM; ISO 11403-1 -2
Charpy Impact Unnotched NBNBDAM; ISO 179/1eU
 NBNB50%RH; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
DAM; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
50%RH; ISO 179/1eU
Charpy Impact, Notched 0.500 J/cm²2.38 ft-lb/in²DAM; ISO 179/1eA
 1.00 J/cm²4.76 ft-lb/in²50%RH; ISO 179/1eA
 0.500 J/cm²
@Temperature -30.0 °C
2.38 ft-lb/in²
@Temperature -22.0 °F
50%RH; ISO 179/1eA
 0.800 J/cm²
@Temperature -30.0 °C
3.81 ft-lb/in²
@Temperature -22.0 °F
DAM; ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 110 µm/m-°C61.1 µin/in-°FDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 115 µm/m-°C63.9 µin/in-°FDAM; ISO 11359-1/-2
Melting Point 203 °C397 °FDAM; 10°C/min; ISO 11357-1/-3
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
DAM; IEC 60695-11-10
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
DAM; IEC 60695-11-10
 
Descriptive Properties
Delivery formPellets
Part Marking Code>PA1010<ISO 11469
ProcessingOther Extrusion
 Profile Extrusion
Regional AvailabilityAsia Pacific
 Europe
 Global
 Near East/Africa
 North America
 South and Central America
Resin IdentificationPA1010ISO 1043
Special characteristicsHeat stabilized or stable to heat
 U.V. stabilized or stable to weather

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Zytel® RS LC1000 BK385 Nylon 1010
Evonik Vestamid® Terra DS 22 natural color Nylon 1010
Suzhou Hipro Polymers Hiprolon® 200 NN Nylon 1010, dry
Suzhou Hipro Polymers Hiprolon® 200 NN Nylon 1010, conditioned
PTS Trimid® N6-200L Nylon 6 with Lube

PZDSY5479a / 234773

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.