MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Celanese Celstran® PA66-GF60-02-US Nylon 66, 60% Glass Reinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 60% Glass Fiber Filled

Material Notes: 60% long glass fiber reinforced, heat stabilized, Nylon 6/6

Information provided by Celanese

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.69 g/cc1.69 g/ccASTM D792
Density 1.69 g/cc0.0611 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.00050 - 0.0010 cm/cm0.00050 - 0.0010 in/inASTM D955
Linear Mold Shrinkage, Transverse 0.0010 - 0.0020 cm/cm0.0010 - 0.0020 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 280 MPa40600 psi5mm/min; ISO 527-2/1A
 318 MPa46100 psiASTM D638
 173 MPa
@Temperature 121 °C
25100 psi
@Temperature 250 °F
ASTM D638
 354 MPa
@Temperature -40.0 °C
51300 psi
@Temperature -40.0 °F
ASTM D638
Elongation at Break 1.7 %1.7 %5mm/min; ISO 527-2/1A
 1.8 %1.8 %ASTM D638
 1.9 %
@Temperature 4.44 °C
1.9 %
@Temperature 40.0 °F
ASTM D638
 2.0 %
@Temperature 80.0 °C
2.0 %
@Temperature 176 °F
ISO 527-1, -2
 2.2 %
@Temperature 121 °C
2.2 %
@Temperature 250 °F
ASTM D638
Tensile Modulus 21.6 GPa3130 ksi50mm/min; ISO 527-2/1A
 23.2 GPa3360 ksiASTM D638
 11.9 GPa
@Temperature 80.0 °C
1730 ksi
@Temperature 176 °F
ISO 527-1, -2
 13.3 GPa
@Temperature 121 °C
1930 ksi
@Temperature 250 °F
ASTM D638
 20.86 GPa
@Temperature -40.0 °C
3025 ksi
@Temperature -40.0 °F
ASTM D638
Flexural Strength 460 MPa66700 psiISO 178
 461 MPa66900 psiASTM D790
 228 MPa
@Temperature 121 °C
33000 psi
@Temperature 250 °F
ASTM D790
 545 MPa
@Temperature -40.0 °C
79000 psi
@Temperature -40.0 °F
ASTM D790
Flexural Modulus 18.7 GPa2710 ksiASTM D790
 19.4 GPa2810 ksiISO 178
 10.3 GPa
@Temperature 121 °C
1490 ksi
@Temperature 250 °F
ASTM D790
 19.3 GPa
@Temperature -40.0 °C
2800 ksi
@Temperature -40.0 °F
ASTM D790
Izod Impact, Notched 6.62 J/cm12.4 ft-lb/inASTM D256
 7.63 J/cm
@Temperature 149 °C
14.3 ft-lb/in
@Temperature 300 °F
ASTM D256
 7.69 J/cm
@Temperature -40.0 °C
14.4 ft-lb/in
@Temperature -40.0 °F
ASTM D256
Charpy Impact, Notched 5.40 J/cm²25.7 ft-lb/in²ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 1.8 MPa (264 psi) 263 °C505 °FASTM D648
 263 °C505 °FISO 75-1, -2
 
Processing PropertiesMetricEnglishComments
Processing Temperature 80.0 - 100 °C176 - 212 °Fcavity
Feed Temperature 20.0 - 50.0 °C68.0 - 122 °F
Zone 1 285 - 295 °C545 - 563 °F
Zone 2 290 - 300 °C554 - 572 °F
Zone 3 300 - 310 °C572 - 590 °F
Zone 4 300 - 315 °C572 - 599 °F
Die Temperature 300 - 315 °C572 - 599 °F
Melt Temperature 300 - 315 °C572 - 599 °F
Drying Temperature 70.0 - 80.0 °C158 - 176 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Moisture Content <= 0.18 %<= 0.18 %
 
Descriptive Properties
Injection moldingYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Bayblend® T88 GF-20 Polycarbonate + SAN Glass Filled Impact Grade
Ensinger TECAPEI® 30% Glass Reinforced, made from Ultem® 2300 PEI
Celanese Celstran® PA66-GF60-02 P11/12 Nylon 66, 60% Glass Reinforced
Celanese Celstran® PA6-GF60-01 Nylon 6, 60% Glass Reinforced
Celanese Celstran® TPU-CF40-01 TPU, 40% Specialty

PHCQ179 / 178634

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.