Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 0.990 g/cc | 0.990 g/cc |
Volatiles | 0.30 % | 0.30 % |
Mooney Viscosity | 41 @Temperature 100 °C | 41 @Temperature 212 °F |
Ash | <= 0.50 % | <= 0.50 % |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Shore A | 45 @Treatment Temp. 25.0 °C, Time 259000 sec | 45 @Treatment Temp. 77.0 °F, Time 72.0 hour |
| 69 @Treatment Temp. 145 °C, Time 1190 sec | 69 @Treatment Temp. 293 °F, Time 0.330 hour |
| 69 @Treatment Temp. 100 °C, Time 259000 sec | 69 @Treatment Temp. 212 °F, Time 72.0 hour |
| 73 @Treatment Temp. 100 °C, Time 259000 sec | 73 @Treatment Temp. 212 °F, Time 72.0 hour |
| 73 @Treatment Temp. 100 °C, Time 259000 sec | 73 @Treatment Temp. 212 °F, Time 72.0 hour |
Tensile Strength at Break | 13.4 MPa @Treatment Temp. 25.0 °C, Time 259000 sec | 1940 psi @Treatment Temp. 77.0 °F, Time 72.0 hour |
| 18.3 MPa @Treatment Temp. 145 °C, Time 1190 sec | 2650 psi @Treatment Temp. 293 °F, Time 0.330 hour |
| 18.8 MPa @Treatment Temp. 100 °C, Time 259000 sec | 2730 psi @Treatment Temp. 212 °F, Time 72.0 hour |
| 18.8 MPa @Treatment Temp. 100 °C, Time 259000 sec | 2730 psi @Treatment Temp. 212 °F, Time 72.0 hour |
| 18.9 MPa @Treatment Temp. 100 °C, Time 259000 sec | 2740 psi @Treatment Temp. 212 °F, Time 72.0 hour |
| 28.3 MPa @Treatment Temp. 145 °C, Time 2990 sec | 4100 psi @Treatment Temp. 293 °F, Time 0.830 hour |
Elongation at Break | 353.1 % @Treatment Temp. 25.0 °C, Time 259000 sec | 353.1 % @Treatment Temp. 77.0 °F, Time 72.0 hour |
| 372.3 % @Treatment Temp. 100 °C, Time 259000 sec | 372.3 % @Treatment Temp. 212 °F, Time 72.0 hour |
| 373.2 % @Treatment Temp. 100 °C, Time 259000 sec | 373.2 % @Treatment Temp. 212 °F, Time 72.0 hour |
| 377 % @Treatment Temp. 100 °C, Time 259000 sec | 377 % @Treatment Temp. 212 °F, Time 72.0 hour |
| 400 % @Treatment Temp. 145 °C, Time 1190 sec | 400 % @Treatment Temp. 293 °F, Time 0.330 hour |
| 575 % @Treatment Temp. 145 °C, Time 2990 sec | 575 % @Treatment Temp. 293 °F, Time 0.830 hour |
300% Modulus | 12.1 MPa @Treatment Temp. 145 °C, Time 2990 sec | 1750 psi @Treatment Temp. 293 °F, Time 0.830 hour |
Rebound | 43.1 % @Temperature 30.0 °C | 43.1 % @Temperature 86.0 °F |
Abrasion | 0.2895 | 0.2895 |
Compression Set | 21.1 % @Temperature 100 °C, Time 259000 sec | 21.1 % @Temperature 212 °F, Time 72.0 hour |
|
Descriptive Properties |
---|
Bound AN Content (%) | 34 |
Color | Tan |
Components | HAF (IRB#7) |
| NBR 6240 |
| Stearic Acid |
| Sulfur |
| TBBS |
| ZnO |
Compound Recipe | Antioxidant(3-C) |
| Antioxidant(RD) |
| Carbon Black(SRF) |
| CZ |
| NBR 6240 |
| Plasticizer(DOP) |
| Stearic Acid |
| Sulfur |
| TT |
| Zinc Oxide |
Rheometer | 1.1 min |
| 1.2 min |
| 1.4 lb-in |
| 2.8 min |
| 23.6 lb-in |
Volume Swell (%) | -2.8 |
| 40.8 |
| -6.8 |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.