MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Sarlink® TPV 24545 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink 24545 is a high performance thermoplastic vulcanizate used in a variety of consumer and industrial applications. This product is a medium hardness, low density, UV stabilized grade suitable for injection molding.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Lap Sealable to PE; Light Stabilized; Low Density; Low Flow; Low Specific Gravity; Lubricated; Medium Hardness; UV Stabilized

Uses: Expansion Joint; Gaskets; Glazing: Grommets; Plugs; Shock Absorbing Pads; Weatherstripping

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³ASTM D792
Melt Flow 2.5 g/10 min
@Load 2.16 kg,
Temperature 230 °C
2.5 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 5050ASTM D2240
 45
@Time 5.00 sec
45
@Time 0.00139 hour
ASTM D2240
Tensile Strength at Break 3.62 MPa525 psiASTM D412
Tensile Stress at Strain 1.52 MPa
@Strain 100 %
220 psi
@Strain 100 %
Elongation at Break 300 %300 %ASTM D412
Tear Strength 14.5 kN/m83.0 pliASTM D624
Compression Set  16 %
@Temperature 22.8 °C,
Time 79200 sec
16 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 32 %
@Temperature 100 °C,
Time 79200 sec
32 %
@Temperature 212 °F,
Time 22.0 hour
ASTM D395
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -60.0 °C-76.0 °FASTM D746
 
Processing PropertiesMetricEnglishComments
Processing Temperature 190 - 230 °C374 - 446 °FInjection, Melt
Rear Barrel Temperature 173 - 213 °C344 - 416 °FInjection
Middle Barrel Temperature 179 - 219 °C354 - 426 °FInjection
Front Barrel Temperature 184 - 224 °C364 - 436 °FInjection
Nozzle Temperature 190 - 230 °C374 - 446 °FInjection
Mold Temperature 35.0 - 60.0 °C95.0 - 140 °FInjection
Back Pressure 0.172 - 0.862 MPa25.0 - 125 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 50 - 120 rpm50 - 120 rpmInjection
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Sarlink® TPV 3470N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV X11059DB Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 6765N Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 2773 Thermoplastic Vulcanizate
Teknor Apex Sarlink® TPV 22035N Thermoplastic Vulcanizate

PTEKNQ1189 / 237680

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.