MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ATI Allegheny Ludlum ALFA-I™ Stainless Steel Type 406  (discontinued **)
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Characteristics:superior oxidation resistance for the temperature range 1600°F-over 2200°F, high electrical resistivity, high resistance to sulfidation, high resistance to carburization.

Applications:automotive exhaust system components, furnace parts, heat exchangers, recuperator parts, kiln lining, refractory reinforcement fibers.

Information provided by Allegheny Ludlum

Key Words: UNS K91470
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.48 g/cc0.270 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 8888
Tensile Strength, Ultimate 519 MPa75300 psiLongitudinal, Unwelded
 524 MPa76000 psi
 538 MPa78000 psiTransverse, Welded
 551 MPa79900 psiLongitudinal, Welded
Tensile Strength, Yield 368 MPa53400 psiLongitudinal, Unwelded
 379 MPa55000 psi
 402 MPa58300 psiTransverse, Welded
 409 MPa59300 psiLongitudinal, Welded
Elongation at Break 28 %28 %in 2"
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.000111 ohm-cm
@Temperature 20.0 °C
0.000111 ohm-cm
@Temperature 68.0 °F
 0.000112 ohm-cm
@Temperature 204 °C
0.000112 ohm-cm
@Temperature 399 °F
 0.000118 ohm-cm
@Temperature 427 °C
0.000118 ohm-cm
@Temperature 801 °F
 0.000129 ohm-cm
@Temperature 649 °C
0.000129 ohm-cm
@Temperature 1200 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.5 µm/m-°C
@Temperature 20.0 - 200 °C
6.39 µin/in-°F
@Temperature 68.0 - 392 °F
 12.8 µm/m-°C
@Temperature 20.0 - 500 °C
7.11 µin/in-°F
@Temperature 68.0 - 932 °F
 14.4 µm/m-°C
@Temperature 20.0 - 1000 °C
8.00 µin/in-°F
@Temperature 68.0 - 1830 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 3.0 %3.0 %
Carbon, C 0.025 %0.025 %
Chromium, Cr 13 %13 %
Iron, Fe 83.24 %83.24 %As Remainder
Manganese, Mn 0.035 %0.035 %
Silicon, Si 0.30 %0.30 %
Titanium, Ti 0.40 %0.40 %

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
406 Stainless Steel
AK Steel 13-4 SR® Ferritic Stainless Steel
ATI Allegheny Ludlum ALFA-II™ Stainless Steel Type 406
ATI Allegheny Ludlum Stainless Steel Ohmaloy® 40 Resistance Alloy
ATI Allegheny Ludlum Ohmaloy® 30 Resistance Alloy

NL1038 / 17806

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.