MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Ineos ABS Lustran® M210TF ABS Pellets  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Molded

Material Notes: Lustran® ABS M210TF is used in general applications for toy and food contact. It meets European standard EN 71, part 3 and ASTM F 963. It has standard impact strength, high gloss, and is easy flowing.

This product was transitioned to the INEOS Styrolution Novodur® trade name. Information provided by the manufacturer.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.04 g/cc0.0376 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0060 cm/cm0.0060 in/inTest Condition: 150x105x3; acc. ISO 2577
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/inTest Condition: 150x105x3; acc. ISO 2577
Melt Flow 30 g/10 min
@Load 10.0 kg,
Temperature 220 °C
30 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 90.0 MPa13100 psiISO 2039-1
Tensile Strength, Yield 42.0 MPa6090 psi50 mm/min; ISO 527-1,-2
Elongation at Break >= 15 %>= 15 %50 mm/min; acc. ISO 527-1,-2
Tensile Modulus 2.05 GPa297 ksi1 mm/min; ISO 527-1,-2
Flexural Strength 62.0 MPa8990 psi2 mm/min; ISO 178
Flexural Modulus 2.05 GPa297 ksi2 mm/min; ISO 178
Izod Impact, Notched (ISO)  11.0 kJ/m²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1A
 17.0 kJ/m²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
Charpy Impact, Notched  1.10 J/cm²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eA
 1.70 J/cm²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+18 ohm-cm1.00e+18 ohm-cmIEC 60093
Surface Resistance 1.00e+16 ohm1.00e+16 ohmIEC 60093
Dielectric Constant  2.9
@Frequency 100 Hz
2.9
@Frequency 100 Hz
IEC 60250
 2.9
@Frequency 1e+6 Hz
2.9
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 35.0 kV/mm
@Thickness 1.00 mm
889 kV/in
@Thickness 0.0394 in
IEC 60243-1
Dissipation Factor  0.0073
@Frequency 100 Hz
0.0073
@Frequency 100 Hz
IEC 60250
 0.0090
@Frequency 1e+6 Hz
0.0090
@Frequency 1e+6 Hz
IEC 60250
 
Thermal PropertiesMetricEnglishComments
CTE, linear 100 µm/m-°C
@Temperature 23.0 - 55.0 °C
55.6 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2; Parallel to Flow
CTE, linear, Transverse to Flow 97.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
53.9 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Deflection Temperature at 0.46 MPa (66 psi) 98.0 °C208 °FISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 94.0 °C201 °FISO 75-1,-2
Vicat Softening Point  95.0 °C
@Load 5.10 kg
203 °F
@Load 11.2 lb
50°C/hour; ISO 306
 98.0 °C
@Load 5.10 kg
208 °F
@Load 11.2 lb
120°C/hour; ISO 306
Flame Spread 63 mm/min2.5 in/min(US-FMVSS); ISO 3795
Glow Wire Flammability Index 700 °C1290 °FIEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Melt Temperature 240 °C464 °FInjection Molding; ISO 294
Mold Temperature 80.0 °C176 °FInjection Molding; ISO 294
Injection Velocity 240 mm/sec9.45 in/secInjection Molding; ISO 294

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ineos ABS Lustran® M205FC ABS Pellets, Injection Molding Grade
Ineos ABS Lustran® M203FC
Denka CL-430 Transparent Resin Polymer (MABS) ABS
SEKISUI SPI ALLEN® 752 ABS
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded

PINEA904 / 107175

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.