MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Nylon 46, Unreinforced
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 46 (PA46); Nylon 46, Unreinforced

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 46, Unreinforced". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.10 - 1.48 g/cc0.0397 - 0.0535 lb/in³Average value: 1.20 g/cc Grade Count:58
Water Absorption 1.20 - 13.5 %1.20 - 13.5 %Average value: 9.09 % Grade Count:17
Moisture Absorption at Equilibrium 2.00 - 3.70 %2.00 - 3.70 %Average value: 3.39 % Grade Count:34
Water Absorption at Saturation 7.00 - 14.0 %7.00 - 14.0 %Average value: 12.4 % Grade Count:7
Viscosity Number 175 - 220 cm³/g1.75 - 2.20 dl/gAverage value: 187 cm³/g Grade Count:7
Linear Mold Shrinkage 0.00330 - 0.0200 cm/cm0.00330 - 0.0200 in/inAverage value: 0.0190 cm/cm Grade Count:31
 0.0190 - 0.0200 cm/cm
@Temperature 80.0 - 80.0 °C
0.0190 - 0.0200 in/in
@Temperature 176 - 176 °F
Average value: 0.0195 cm/cm Grade Count:4
Linear Mold Shrinkage, Transverse 0.0150 - 0.0200 cm/cm0.0150 - 0.0200 in/inAverage value: 0.0197 cm/cm Grade Count:17
 0.0190 - 0.0200 cm/cm
@Temperature 80.0 - 80.0 °C
0.0190 - 0.0200 in/in
@Temperature 176 - 176 °F
Average value: 0.0195 cm/cm Grade Count:4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 90.0 - 10090.0 - 100Average value: 95.0 Grade Count:4
Hardness, Shore D 80.0 - 84.080.0 - 84.0Average value: 82.0 Grade Count:4
Ball Indentation Hardness 165 - 200 MPa23900 - 29000 psiAverage value: 173 MPa Grade Count:3
Tensile Strength, Ultimate 65.0 - 197 MPa9430 - 28500 psiAverage value: 102 MPa Grade Count:5
Tensile Strength, Yield 45.0 - 105 MPa6530 - 15200 psiAverage value: 73.4 MPa Grade Count:51
 30.0 - 50.0 MPa
@Temperature 120 - 200 °C
4350 - 7250 psi
@Temperature 248 - 392 °F
Average value: 38.3 MPa Grade Count:8
Elongation at Break 2.80 - 280 %2.80 - 280 %Average value: 44.2 % Grade Count:41
 >= 50.0 %
@Temperature 120 - 200 °C
>= 50.0 %
@Temperature 248 - 392 °F
Average value: 50.0 % Grade Count:8
Elongation at Yield 5.00 - 55.0 %5.00 - 55.0 %Average value: 29.8 % Grade Count:29
Modulus of Elasticity 0.600 - 12.1 GPa87.0 - 1750 ksiAverage value: 2.31 GPa Grade Count:53
 0.350 - 0.800 GPa
@Temperature 120 - 200 °C
50.8 - 116 ksi
@Temperature 248 - 392 °F
Average value: 0.622 GPa Grade Count:8
Flexural Yield Strength 103 - 283 MPa15000 - 41000 psiAverage value: 138 MPa Grade Count:8
Flexural Modulus 0.550 - 11.4 GPa79.8 - 1650 ksiAverage value: 2.60 GPa Grade Count:23
 0.350 - 0.800 GPa
@Temperature 120 - 160 °C
50.8 - 116 ksi
@Temperature 248 - 320 °F
Average value: 0.659 GPa Grade Count:8
Izod Impact, Notched 0.267 - 0.801 J/cm0.500 - 1.50 ft-lb/inAverage value: 0.679 J/cm Grade Count:7
 0.74746 - 0.74746 J/cm
@Temperature -40.0 - -40.0 °C
1.4003 - 1.4003 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 0.747 J/cm Grade Count:2
 0.74746 - 0.74746 J/cm
@Thickness 3.17 - 3.17 mm
1.4003 - 1.4003 ft-lb/in
@Thickness 0.125 - 0.125 in
Average value: 0.747 J/cm Grade Count:2
Izod Impact, Unnotched 4.27 - 5340 J/cm8.00 - 10000 ft-lb/inAverage value: 7.65 J/cm Grade Count:5
Izod Impact, Notched (ISO) 6.00 - 125 kJ/m²2.86 - 59.5 ft-lb/in²Average value: 29.1 kJ/m² Grade Count:16
 4.00 - 40.0 kJ/m²
@Temperature -40.0 - -30.0 °C
1.90 - 19.0 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 8.63 kJ/m² Grade Count:13
Charpy Impact Unnotched 8.50 J/cm² - NB40.5 ft-lb/in² - NBAverage value: 9.25 J/cm² Grade Count:40
 8.50 J/cm² - NB
@Temperature -30.0 - -30.0 °C
40.5 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 10.1 J/cm² Grade Count:37
Charpy Impact, Notched 0.400 J/cm² - NB1.90 ft-lb/in² - NBAverage value: 3.09 J/cm² Grade Count:48
 0.300 - 3.00 J/cm²
@Temperature -30.0 - -30.0 °C
1.43 - 14.3 ft-lb/in²
@Temperature -22.0 - -22.0 °F
Average value: 1.00 J/cm² Grade Count:36
Tensile Creep Modulus, 1000 hours 500 - 850 MPa72500 - 123000 psiAverage value: 570 MPa Grade Count:5
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1000 - 1.00e+15 ohm-cm1000 - 1.00e+15 ohm-cmAverage value: 2.32e+14 ohm-cm Grade Count:46
Surface Resistance 1.00e+6 - 1.00e+16 ohm1.00e+6 - 1.00e+16 ohmAverage value: 1.84e+15 ohm Grade Count:10
Dielectric Constant 3.20 - 22.03.20 - 22.0Average value: 6.53 Grade Count:12
Dielectric Strength 10.0 - 30.0 kV/mm254 - 762 kV/inAverage value: 20.9 kV/mm Grade Count:40
Dissipation Factor 0.000500 - 0.1300.000500 - 0.130Average value: 0.0265 Grade Count:9
Dielectric Loss Index 0.00900 - 0.3500.00900 - 0.350Average value: 0.105 Grade Count:3
Comparative Tracking Index 325 - 600 V325 - 600 VAverage value: 436 V Grade Count:31
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.0 - 160 µm/m-°C10.0 - 88.9 µin/in-°FAverage value: 85.1 µm/m-°C Grade Count:33
CTE, linear, Transverse to Flow 20.0 - 180 µm/m-°C11.1 - 100 µin/in-°FAverage value: 105 µm/m-°C Grade Count:23
Thermal Conductivity 0.300 - 0.303 W/m-K2.08 - 2.10 BTU-in/hr-ft²-°FAverage value: 0.301 W/m-K Grade Count:4
Melting Point 290 - 295 °C554 - 563 °FAverage value: 295 °C Grade Count:43
Maximum Service Temperature, Air 128 - 280 °C262 - 536 °FAverage value: 166 °C Grade Count:6
Deflection Temperature at 0.46 MPa (66 psi) 200 - 290 °C392 - 554 °FAverage value: 261 °C Grade Count:11
Deflection Temperature at 1.8 MPa (264 psi) 90.0 - 285 °C194 - 545 °FAverage value: 174 °C Grade Count:36
Vicat Softening Point 250 - 290 °C482 - 554 °FAverage value: 283 °C Grade Count:7
Minimum Service Temperature, Air -40.0 °C-40.0 °FAverage value: -40.0 °C Grade Count:4
Glass Transition Temp, Tg 75.0 - 80.0 °C167 - 176 °FAverage value: 75.6 °C Grade Count:9
Flammability, UL94 HB - V-0HB - V-0Grade Count:26
Oxygen Index 27.0 - 29.0 %27.0 - 29.0 %Average value: 27.5 % Grade Count:4
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 - 327 °C536 - 620 °FAverage value: 303 °C Grade Count:3
Mold Temperature 65.6 - 149 °C150 - 300 °FAverage value: 103 °C Grade Count:5
Drying Temperature 80.0 - 121 °C176 - 250 °FAverage value: 93.7 °C Grade Count:3
Moisture Content 0.0300 - 0.0800 %0.0300 - 0.0800 %Average value: 0.0533 % Grade Count:3
Injection Pressure 68.9 - 103 MPa10000 - 15000 psiAverage value: 86.2 MPa Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Unreinforced
Overview of materials for Nylon 66, Unreinforced
Overview of materials for Polyetheretherketone, Unreinforced
Overview of materials for Nylon 11, Unreinforced
Overview of materials for Nylon 612, Unreinforced

O2390 / 77957

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.