MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 5056-H38
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A95056; ISO AlMg5; ISO AlMg5Cr; Aluminium 5056-H38; AA5056-H38; Al5056-H38
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 2.64 g/cc0.0954 lb/in³AA; Typical
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 100100AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 126126Converted from Brinell Hardness Value
Hardness, Rockwell A 4141Converted from Brinell Hardness Value
Hardness, Rockwell B 6363Converted from Brinell Hardness Value
Hardness, Vickers 112112Converted from Brinell Hardness Value
Tensile Strength, Ultimate 414 MPa60000 psiAA; Typical
 41.0 MPa
@Temperature 371 °C
5950 psi
@Temperature 700 °F
 76.0 MPa
@Temperature 316 °C
11000 psi
@Temperature 601 °F
 110 MPa
@Temperature 260 °C
16000 psi
@Temperature 500 °F
 179 MPa
@Temperature 204 °C
26000 psi
@Temperature 399 °F
 262 MPa
@Temperature 149 °C
38000 psi
@Temperature 300 °F
 414 MPa
@Temperature 24.0 °C
60000 psi
@Temperature 75.2 °F
Tensile Strength, Yield 345 MPa50000 psiAA; Typical
 28.0 MPa
@Temperature 371 °C
4060 psi
@Temperature 700 °F
 48.0 MPa
@Temperature 316 °C
6960 psi
@Temperature 601 °F
 69.0 MPa
@Temperature 260 °C
10000 psi
@Temperature 500 °F
 124 MPa
@Temperature 204 °C
18000 psi
@Temperature 399 °F
 214 MPa
@Temperature 149 °C
31000 psi
@Temperature 300 °F
 345 MPa
@Temperature 24.0 °C
50000 psi
@Temperature 75.2 °F
Elongation at Break  15 %
@Temperature 24.0 °C
15 %
@Temperature 75.2 °F
 30 %
@Temperature 149 °C
30 %
@Temperature 300 °F
 50 %
@Temperature 204 °C
50 %
@Temperature 399 °F
 80 %
@Temperature 260 °C
80 %
@Temperature 500 °F
 100 %
@Temperature 316 °C
100 %
@Temperature 601 °F
 130 %
@Temperature 371 °C
130 %
@Temperature 700 °F
 15 %
@Diameter 12.7 mm
15 %
@Diameter 0.500 in
AA; Typical
Modulus of Elasticity 71.0 GPa10300 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Poissons Ratio 0.330.33Estimated from trends in similar Al alloys.
Fatigue Strength 152 MPa
@# of Cycles 5.00e+8
22000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 25.9 GPa3760 ksi
Shear Strength 221 MPa32000 psiAA; Typical
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000632 ohm-cm
@Temperature 20.0 °C
0.00000632 ohm-cm
@Temperature 68.0 °F
AA; Typical
 
Thermal PropertiesMetricEnglishComments
CTE, linear  22.5 µm/m-°C
@Temperature -50.0 - 20.0 °C
12.5 µin/in-°F
@Temperature -58.0 - 68.0 °F
 24.1 µm/m-°C
@Temperature 20.0 - 100 °C
13.4 µin/in-°F
@Temperature 68.0 - 212 °F
AA; Typical; average over range
 25.2 µm/m-°C
@Temperature 20.0 - 200 °C
14.0 µin/in-°F
@Temperature 68.0 - 392 °F
 26.1 µm/m-°C
@Temperature 20.0 - 300 °C
14.5 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.904 J/g-°C0.216 BTU/lb-°F
Thermal Conductivity 108 W/m-K750 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 568.3 - 638 °C1055 - 1180 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness
Solidus 568.3 °C1055 °FAA; Typical
Liquidus 638 °C1180 °FAA; Typical
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 413 °C775 °Fholding at temperature not required
Hot-Working Temperature 316 - 482 °C600 - 900 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 92.9 - 95.4 %92.9 - 95.4 %As remainder
Chromium, Cr 0.05 - 0.20 %0.05 - 0.20 %
Copper, Cu <= 0.10 %<= 0.10 %
Iron, Fe <= 0.40 %<= 0.40 %
Magnesium, Mg 4.5 - 5.6 %4.5 - 5.6 %
Manganese, Mn 0.05 - 0.20 %0.05 - 0.20 %
Other, each <= 0.05 %<= 0.05 %
Other, total <= 0.15 %<= 0.15 %
Silicon, Si <= 0.30 %<= 0.30 %
Zinc, Zn <= 0.10 %<= 0.10 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum 5056-H18
Aluminum 5056-O
5754-H24 Aluminum
Aluminum 5052-H38
Aluminum 5052-H32

MA5056H38 / 9167

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.