MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Thermoset Polyester Glass SMC
Categories: Polymer; Thermoset; Polyester, TS; Thermoset Polyester Glass SMC

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Thermoset Polyester Glass SMC". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.810 - 2.01 g/cc0.0293 - 0.0726 lb/in³Average value: 1.77 g/cc Grade Count:203
Filler Content 18.0 - 40.0 %18.0 - 40.0 %Average value: 25.9 % Grade Count:32
Water Absorption 0.000 - 1.10 %0.000 - 1.10 %Average value: 0.294 % Grade Count:163
 1.20 - 1.20 %
@Temperature 50.0 - 50.0 °C
1.20 - 1.20 %
@Temperature 122 - 122 °F
Average value: 1.20 % Grade Count:1
 1.20 - 1.20 %
@Time 3.60e+6 - 3.60e+6 sec
1.20 - 1.20 %
@Time 1000 - 1000 hour
Average value: 1.20 % Grade Count:1
Linear Mold Shrinkage -0.00100 - 0.0200 cm/cm-0.00100 - 0.0200 in/inAverage value: 0.00107 cm/cm Grade Count:149
 
Mechanical PropertiesMetricEnglishComments
Hardness, Barcol 15.0 - 74.015.0 - 74.0Average value: 49.5 Grade Count:73
Hardness, Rockwell M 70.0 - 11670.0 - 116Average value: 87.0 Grade Count:25
Tensile Strength, Ultimate 13.0 - 2590 MPa1890 - 376000 psiAverage value: 101 MPa Grade Count:174
 64.0 - 64.0 MPa
@Temperature 150 - 150 °C
9280 - 9280 psi
@Temperature 302 - 302 °F
Average value: 64.0 MPa Grade Count:1
Tensile Strength, Yield 13.0 - 160 MPa1890 - 23200 psiAverage value: 72.7 MPa Grade Count:33
Elongation at Break 0.000 - 1.80 %0.000 - 1.80 %Average value: 0.570 % Grade Count:43
Modulus of Elasticity 2.76 - 88.2 GPa400 - 12800 ksiAverage value: 12.5 GPa Grade Count:116
 9.30 - 9.30 GPa
@Temperature 150 - 150 °C
1350 - 1350 ksi
@Temperature 302 - 302 °F
Average value: 9.30 GPa Grade Count:1
Flexural Yield Strength 50.0 - 1000 MPa7250 - 145000 psiAverage value: 179 MPa Grade Count:208
 108 - 557.096 MPa
@Temperature 120 - 160 °C
15700 - 80800.1 psi
@Temperature 248 - 320 °F
Average value: 269 MPa Grade Count:2
 65.0 - 65.0 MPa
@Temperature 130 - 130 °C
9430 - 9430 psi
@Temperature 266 - 266 °F
Average value: 269 MPa Grade Count:1
 65.0 - 65.0 MPa
@Thickness >=1.50 mm
9430 - 9430 psi
@Thickness >=0.0591 in
Average value: 269 MPa Grade Count:1
Flexural Modulus 3.00 - 55.2 GPa435 - 8000 ksiAverage value: 10.6 GPa Grade Count:189
 8.00 - 27.0 GPa
@Temperature 120 - 160 °C
1160 - 3920 ksi
@Temperature 248 - 320 °F
Average value: 20.3 GPa Grade Count:2
Compressive Yield Strength 74.5 - 379 MPa10800 - 55000 psiAverage value: 180 MPa Grade Count:95
Compressive Modulus 6.89 - 17.2 GPa1000 - 2500 ksiAverage value: 10.3 GPa Grade Count:8
Ultimate Bearing Strength 221 MPa32000 psiAverage value: 221 MPa Grade Count:6
Poissons Ratio 0.3000.300Average value: 0.300 Grade Count:66
Shear Modulus 1.30 - 5.80 GPa189 - 841 ksiAverage value: 4.09 GPa Grade Count:66
Shear Strength 31.0 - 124 MPa4500 - 18000 psiAverage value: 67.7 MPa Grade Count:23
 33.7843 - 39.9896 MPa
@Temperature 120 - 160 °C
4900.01 - 5800.01 psi
@Temperature 248 - 320 °F
Average value: 36.9 MPa Grade Count:1
Izod Impact, Notched 0.640 - 26.7 J/cm1.20 - 50.0 ft-lb/inAverage value: 7.65 J/cm Grade Count:129
Izod Impact, Unnotched 3.20 - 15.0 J/cm6.00 - 28.1 ft-lb/inAverage value: 9.08 J/cm Grade Count:54
Charpy Impact Unnotched 5.00 - 60.0 J/cm²23.8 - 286 ft-lb/in²Average value: 9.71 J/cm² Grade Count:23
Charpy Impact, Notched 1.90 - 17.0 J/cm²9.04 - 80.9 ft-lb/in²Average value: 7.05 J/cm² Grade Count:42
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+11 - 1.00e+16 ohm-cm1.00e+11 - 1.00e+16 ohm-cmAverage value: 1.04e+15 ohm-cm Grade Count:44
Surface Resistance 1e+05 - 1.00e+14 ohm1e+05 - 1.00e+14 ohmAverage value: 3.21e+13 ohm Grade Count:54
Dielectric Constant 4.00 - 5.204.00 - 5.20Average value: 4.31 Grade Count:54
Dielectric Strength 1.38 - 47.2 kV/mm35.0 - 1200 kV/inAverage value: 16.8 kV/mm Grade Count:113
 1.85039 - 23.0 kV/mm
@Temperature 90.0 - 90.0 °C
46.9999 - 584 kV/in
@Temperature 194 - 194 °F
Average value: 10.9 kV/mm Grade Count:2
 2.3622 - 10.0 kV/mm
@Temperature 90.0 - 90.0 °C
60.000 - 254 kV/in
@Temperature 194 - 194 °F
Average value: 10.9 kV/mm Grade Count:1
 2.3622 - 10.0 kV/mm
@Thickness 3.00 - 3.00 mm
60.000 - 254 kV/in
@Thickness 0.118 - 0.118 in
Average value: 10.9 kV/mm Grade Count:1
Dielectric Breakdown 54000 - 60000 V54000 - 60000 VAverage value: 56000 V Grade Count:4
Dissipation Factor 0.00300 - 0.06000.00300 - 0.0600Average value: 0.0152 Grade Count:48
Arc Resistance 100 - 194 sec100 - 194 secAverage value: 169 sec Grade Count:77
Comparative Tracking Index 500 - 601 V500 - 601 VAverage value: 593 V Grade Count:67
 
Thermal PropertiesMetricEnglishComments
CTE, linear -1.02 - 36.0 µm/m-°C-0.567 - 20.0 µin/in-°FAverage value: 21.2 µm/m-°C Grade Count:82
CTE, linear, Transverse to Flow 20.0 - 27.0 µm/m-°C11.1 - 15.0 µin/in-°FAverage value: 25.0 µm/m-°C Grade Count:33
Specific Heat Capacity 1.10 - 1.51 J/g-°C0.263 - 0.360 BTU/lb-°FAverage value: 1.13 J/g-°C Grade Count:38
Thermal Conductivity 0.250 - 0.700 W/m-K1.74 - 4.86 BTU-in/hr-ft²-°FAverage value: 0.486 W/m-K Grade Count:73
Maximum Service Temperature, Air 130 - 300 °C266 - 572 °FAverage value: 176 °C Grade Count:65
Maximum Service Temperature, Inert 130 - 180 °C266 - 356 °FAverage value: 157 °C Grade Count:3
Deflection Temperature at 1.8 MPa (264 psi) 150 - 260 °C302 - 500 °FAverage value: 213 °C Grade Count:102
Minimum Service Temperature, Air -40.0 °C-40.0 °FAverage value: -40.0 °C Grade Count:33
Glass Transition Temp, Tg 125 - 210 °C257 - 410 °FAverage value: 171 °C Grade Count:34
UL RTI, Electrical 120 - 160 °C248 - 320 °FAverage value: 131 °C Grade Count:28
UL RTI, Mechanical with Impact 130 - 150 °C266 - 302 °FAverage value: 131 °C Grade Count:26
UL RTI, Mechanical without Impact 130 - 160 °C266 - 320 °FAverage value: 132 °C Grade Count:27
Flammability, UL94 HB - 5VAHB - 5VAGrade Count:115
Flame Spread Index 12.9 - 25.012.9 - 25.0Average value: 20.1 Grade Count:8
Smoke Density 600 - 700600 - 700Average value: 650 Grade Count:3
Oxygen Index 20.0 - 70.0 %20.0 - 70.0 %Average value: 26.4 % Grade Count:33
Glow Wire Test 690 - 960 °C1270 - 1760 °FAverage value: 830 °C Grade Count:41
 
Processing PropertiesMetricEnglishComments
Processing Temperature 120 - 160 °C248 - 320 °FAverage value: 147 °C Grade Count:69
Mold Temperature 140 - 160 °C284 - 320 °FAverage value: 150 °C Grade Count:23
Cure Time 120 - 120 min
@Temperature 200 - 200 °C
2.00 - 2.00 hour
@Temperature 392 - 392 °F
Average value: 188 min Grade Count:1
 960 - 960 min
@Temperature 80.0 - 80.0 °C
16.0 - 16.0 hour
@Temperature 176 - 176 °F
Average value: 188 min Grade Count:1
 960 - 960 min
@Pressure 0.621 - 0.621 MPa
16.0 - 16.0 hour
@Pressure 90.0 - 90.0 psi
Average value: 188 min Grade Count:1
 1.25 - 5.00 min
@Temperature 138 - 149 °C
0.0208 - 0.0833 hour
@Temperature 280 - 300 °F
Average value: 188 min Grade Count:4
 1.25 - 5.00 min
@Thickness 1.52 - 6.35 mm
0.0208 - 0.0833 hour
@Thickness 0.0600 - 0.250 in
Average value: 188 min Grade Count:4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Thermoset Polyester Glass Filled BMC
Applied Composites 120 Polyester SMC
Overview of materials for Polyester (Thermoset) - Rigid
Overview of materials for Thermoset Polyurethane, Elastomer, Unreinforced
Overview of materials for Polyester Thermoplastic Elastomer, Glass Filled

O3510 / 78219

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.