MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI 1040 Steel, annealed at 790°C (1450°F), furnace cooled 11°C (20°F) per hour to 650°C (1200°F), air cooled, 25 mm (1 in.) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: Typical uses include machine, plow, and carriage bolts, tie wire, cylinder head studs, and machined parts, U-bolts, concrete reinforcing rods, forgings, and non-critical springs.

Key Words: UNS G10400, ASTM A29, ASTM A108, ASTM A510, ASTM A519, ASTM A546, ASTM A576, ASTM A682, MIL SPEC MIL-S-11310 (CS1040), SAE J403, SAE J412, SAE J414, DIN 1.1186, JIS S 40 C, BS 970 060A40, BS 970 080A40, BS 970 080M40 (EN8), BS 2 S 93
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.845 g/cc0.2834 lb/in³Chemical composition of 0.435% C, 0.69% Mn, 0.20% Si, annealed at 860°C (1580°F).
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 149149
Hardness, Knoop 169169Converted from Brinell
Hardness, Rockwell B 8080Converted from Brinell
Hardness, Vickers 155155Converted from Brinell
Tensile Strength, Ultimate 519 MPa75300 psi
Tensile Strength, Yield 353 MPa51200 psi
Elongation at Break 30.2 %30.2 %in 50 mm
Reduction of Area 57.2 %57.2 %
Modulus of Elasticity 200 GPa29000 ksiTypical for steel
Bulk Modulus 160 GPa23200 ksiTypical for steels
Poissons Ratio 0.290.29Typical For Steel
Shear Modulus 80.0 GPa11600 ksiTypical for steels
Izod Impact 45.0 J33.2 ft-lbannealed at 790°C (1450°F)
 49.0 J36.1 ft-lbas rolled
 65.0 J47.9 ft-lbnormalized at 900°C (1650°F)
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000171 ohm-cm
@Temperature 20.0 °C
0.0000171 ohm-cm
@Temperature 68.0 °F
 0.0000221 ohm-cm
@Temperature 100 °C
0.0000221 ohm-cm
@Temperature 212 °F
 0.0000296 ohm-cm
@Temperature 200 °C
0.0000296 ohm-cm
@Temperature 392 °F
 0.0000493 ohm-cm
@Temperature 400 °C
0.0000493 ohm-cm
@Temperature 752 °F
 0.0000763 ohm-cm
@Temperature 600 °C
0.0000763 ohm-cm
@Temperature 1110 °F
 0.0000932 ohm-cm
@Temperature 700 °C
0.0000932 ohm-cm
@Temperature 1290 °F
 0.0001111 ohm-cm
@Temperature 800 °C
0.0001111 ohm-cm
@Temperature 1470 °F
 0.0001149 ohm-cm
@Temperature 900 °C
0.0001149 ohm-cm
@Temperature 1650 °F
 0.0001179 ohm-cm
@Temperature 1000 °C
0.0001179 ohm-cm
@Temperature 1830 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.3 µm/m-°C
@Temperature 20.0 - 100 °C
6.28 µin/in-°F
@Temperature 68.0 - 212 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu.
 12.1 µm/m-°C
@Temperature 20.0 - 200 °C
6.72 µin/in-°F
@Temperature 68.0 - 392 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu.
 12.2 µm/m-°C
@Temperature 20.0 - 300 °C
6.78 µin/in-°F
@Temperature 68.0 - 572 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 13.3 µm/m-°C
@Temperature 20.0 - 400 °C
7.39 µin/in-°F
@Temperature 68.0 - 752 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 13.9 µm/m-°C
@Temperature 20.0 - 500 °C
7.72 µin/in-°F
@Temperature 68.0 - 932 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 14.2 µm/m-°C
@Temperature 20.0 - 600 °C
7.89 µin/in-°F
@Temperature 68.0 - 1110 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 14.8 µm/m-°C
@Temperature 20.0 - 700 °C
8.22 µin/in-°F
@Temperature 68.0 - 1290 °F
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
Specific Heat Capacity  0.486 J/g-°C
@Temperature >=100 °C
0.116 BTU/lb-°F
@Temperature >=212 °F
 0.515 J/g-°C
@Temperature 150 - 200 °C
0.123 BTU/lb-°F
@Temperature 302 - 392 °F
 0.528 J/g-°C
@Temperature 200 - 250 °C
0.126 BTU/lb-°F
@Temperature 392 - 482 °F
 0.548 J/g-°C
@Temperature 250 - 300 °C
0.131 BTU/lb-°F
@Temperature 482 - 572 °F
 0.569 J/g-°C
@Temperature 300 - 350 °C
0.136 BTU/lb-°F
@Temperature 572 - 662 °F
 0.586 J/g-°C
@Temperature 350 - 400 °C
0.140 BTU/lb-°F
@Temperature 662 - 752 °F
 0.624 J/g-°C
@Temperature 750 - 800 °C
0.149 BTU/lb-°F
@Temperature 1380 - 1470 °F
 0.649 J/g-°C
@Temperature 450 - 500 °C
0.155 BTU/lb-°F
@Temperature 842 - 932 °F
 0.708 J/g-°C
@Temperature 550 - 600 °C
0.169 BTU/lb-°F
@Temperature 1020 - 1110 °F
 0.770 J/g-°C
@Temperature 650 - 700 °C
0.184 BTU/lb-°F
@Temperature 1200 - 1290 °F
 1.583 J/g-°C
@Temperature 700 - 750 °C
0.3783 BTU/lb-°F
@Temperature 1290 - 1380 °F
Thermal Conductivity  24.7 W/m-K
@Temperature 800 °C
171 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 29.8 W/m-K
@Temperature 1200 °C
207 BTU-in/hr-ft²-°F
@Temperature 2190 °F
 30.1 W/m-K
@Temperature 700 °C
209 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 32.9 W/m-K
@Temperature 1000 °C
228 BTU-in/hr-ft²-°F
@Temperature 1830 °F
 33.9 W/m-K
@Temperature 600 °C
235 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 38.2 W/m-K
@Temperature 500 °C
265 BTU-in/hr-ft²-°F
@Temperature 932 °F
 41.7 W/m-K
@Temperature 400 °C
289 BTU-in/hr-ft²-°F
@Temperature 752 °F
 45.7 W/m-K
@Temperature 300 °C
317 BTU-in/hr-ft²-°F
@Temperature 572 °F
 48.1 W/m-K
@Temperature 200 °C
334 BTU-in/hr-ft²-°F
@Temperature 392 °F
 50.7 W/m-K
@Temperature 100 °C
352 BTU-in/hr-ft²-°F
@Temperature 212 °F
 51.9 W/m-K
@Temperature 0.000 °C
360 BTU-in/hr-ft²-°F
@Temperature 32.0 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.37 - 0.44 %0.37 - 0.44 %
Iron, Fe 98.6 - 99 %98.6 - 99 %As remainder
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S <= 0.050 %<= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1040 Steel, normalized at 900°C (1650°F)
AISI 1040 Steel, annealed at 790°C (1450°F)
AISI 1040 Steel, as rolled
AISI 1040 Steel, normalized at 900°C (1650°F), air cooled, 13 mm (0.5 in.) round
MetalTek WCC Cast 105-85 Alloy Steel

M104AR / 6968

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.