MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
AISI 1040 Steel, annealed at 790°C (1450°F), furnace cooled 11°C (20°F) per hour to 650°C (1200°F), air cooled, 25 mm (1 in.) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Medium Carbon Steel

Material Notes: Typical uses include machine, plow, and carriage bolts, tie wire, cylinder head studs, and machined parts, U-bolts, concrete reinforcing rods, forgings, and non-critical springs.

Key Words: UNS G10400, ASTM A29, ASTM A108, ASTM A510, ASTM A519, ASTM A546, ASTM A576, ASTM A682, MIL SPEC MIL-S-11310 (CS1040), SAE J403, SAE J412, SAE J414, DIN 1.1186, JIS S 40 C, BS 970 060A40, BS 970 080A40, BS 970 080M40 (EN8), BS 2 S 93
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.845 g/ccChemical composition of 0.435% C, 0.69% Mn, 0.20% Si, annealed at 860°C (1580°F).
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 149
Hardness, Knoop 169Converted from Brinell
Hardness, Rockwell B 80Converted from Brinell
Hardness, Vickers 155Converted from Brinell
Tensile Strength, Ultimate 519 MPa
Tensile Strength, Yield 353 MPa
Elongation at Break 30.2 %in 50 mm
Reduction of Area 57.2 %
Modulus of Elasticity 200 GPaTypical for steel
Bulk Modulus 160 GPaTypical for steels
Poissons Ratio 0.29Typical For Steel
Shear Modulus 80.0 GPaTypical for steels
Izod Impact 45.0 Jannealed at 790°C (1450°F)
 49.0 Jas rolled
 65.0 Jnormalized at 900°C (1650°F)
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000171 ohm-cm
@Temperature 20.0 °C
 0.0000221 ohm-cm
@Temperature 100 °C
 0.0000296 ohm-cm
@Temperature 200 °C
 0.0000493 ohm-cm
@Temperature 400 °C
 0.0000763 ohm-cm
@Temperature 600 °C
 0.0000932 ohm-cm
@Temperature 700 °C
 0.0001111 ohm-cm
@Temperature 800 °C
 0.0001149 ohm-cm
@Temperature 900 °C
 0.0001179 ohm-cm
@Temperature 1000 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.3 µm/m-°C
@Temperature 20.0 - 100 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu.
 12.1 µm/m-°C
@Temperature 20.0 - 200 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu.
 12.2 µm/m-°C
@Temperature 20.0 - 300 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 13.3 µm/m-°C
@Temperature 20.0 - 400 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 13.9 µm/m-°C
@Temperature 20.0 - 500 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 14.2 µm/m-°C
@Temperature 20.0 - 600 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
 14.8 µm/m-°C
@Temperature 20.0 - 700 °C
Composition of 0.40% C, 0.11% Mn, 0.01% P, 0.03% S, 0.03% Si, 0.03% Cu
Specific Heat Capacity 0.486 J/g-°C
@Temperature >=100 °C
 0.515 J/g-°C
@Temperature 150 - 200 °C
 0.528 J/g-°C
@Temperature 200 - 250 °C
 0.548 J/g-°C
@Temperature 250 - 300 °C
 0.569 J/g-°C
@Temperature 300 - 350 °C
 0.586 J/g-°C
@Temperature 350 - 400 °C
 0.624 J/g-°C
@Temperature 750 - 800 °C
 0.649 J/g-°C
@Temperature 450 - 500 °C
 0.708 J/g-°C
@Temperature 550 - 600 °C
 0.770 J/g-°C
@Temperature 650 - 700 °C
 1.583 J/g-°C
@Temperature 700 - 750 °C
Thermal Conductivity 24.7 W/m-K
@Temperature 800 °C
 29.8 W/m-K
@Temperature 1200 °C
 30.1 W/m-K
@Temperature 700 °C
 32.9 W/m-K
@Temperature 1000 °C
 33.9 W/m-K
@Temperature 600 °C
 38.2 W/m-K
@Temperature 500 °C
 41.7 W/m-K
@Temperature 400 °C
 45.7 W/m-K
@Temperature 300 °C
 48.1 W/m-K
@Temperature 200 °C
 50.7 W/m-K
@Temperature 100 °C
 51.9 W/m-K
@Temperature 0.000 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.37 - 0.44 %
Iron, Fe 98.6 - 99 %As remainder
Manganese, Mn 0.60 - 0.90 %
Phosphorus, P <= 0.040 %
Sulfur, S <= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 1040 Steel, normalized at 900°C (1650°F)
AISI 1040 Steel, annealed at 790°C (1450°F)
AISI 1040 Steel, as rolled
AISI 1040 Steel, normalized at 900°C (1650°F), air cooled, 13 mm (0.5 in.) round
MetalTek WCC Cast 105-85 Alloy Steel

M104AR / 6968

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.