MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

NatureWorks® Ingeo™ 2002D Extrusion Grade PLA  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polylactic Acid (PLA) Biopolymer

Material Notes: NatureWorks® PLA polymer 2002D is a thermoplastic resin derived from annually renewable resources and is specifically designed for extrusion/thermoforming applications. PLA polymer 2002D is a clear extrusion sheet grade and processes easily on conventional extrusion and thermoforming equipment.

Potential applications for PLA polymer 2002D include: Dairy containers; Food serviceware; Transparent food containers; Blister packaging; Cold drink cups

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.24 g/cc1.24 g/ccASTM D792
Melt Flow 5.0 - 7.0 g/10 min
@Load 2.16 kg,
Temperature 210 °C
5.0 - 7.0 g/10 min
@Load 4.76 lb,
Temperature 410 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 53.0 MPa7690 psiASTM D882
Tensile Strength, Yield 60.0 MPa8700 psiASTM D882
Elongation at Break 6.0 %6.0 %ASTM D882
Tensile Modulus 3.45 GPa500 ksiASTM D882
Izod Impact, Notched 0.1281 J/cm0.2400 ft-lb/inASTM D256
 
Optical PropertiesMetricEnglishComments
Transmission, Visible 90 %90 %Thickness Unknown
 
Processing PropertiesMetricEnglishComments
Feed Temperature 180 °C356 °F
Adapter Temperature 200 °C392 °F
Die Temperature 190 °C374 °F
Melt Temperature 210 °C410 °F
Drying Temperature 90.0 °C
@Time 7200 sec
194 °F
@Time 2.00 hour
Moisture Content <= 0.025 %<= 0.025 %
Dew Point -40.0 °C-40.0 °F
Drying Air Flow Rate >= 14.2 l/min>= 0.500 ft³/min (CFM)
Screw Speed 20 - 100 rpm20 - 100 rpm

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polylactic Acid (PLA) Biopolymer
NatureWorks® Ingeo™ AW 300D Injection Grade Biopolymer
NatureWorks® Ingeo™ 3001D Injection Grade PLA
NatureWorks® Ingeo™ 2003D General Purpose Transparent Extrusion Grade Biopolymer
NatureWorks® Ingeo™ 3251D Injection Grade PLA

PNATU80 / 103478

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.