MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type S14800 Stainless Steel condition SRH950, vacuum induction melted
Categories: Metal; Ferrous Metal; Stainless Steel; Precipitation Hardening Stainless; T S10000 Series Stainless Steel

Material Notes: Specimens were vacuum induction melted, tested in transverse, 25 mm wide, 6.4 mm thick, with an edge notch-root radius of 0.018 mm.

Key Words: UNS S14800, AMS 5601, AMS 5603; Precipitation Hardening
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.70 g/cc0.278 lb/in³In condition SRH950, 7.83 in condition A
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1502 MPa217800 psi
 1252 MPa
@Temperature 345 °C
181600 psi
@Temperature 653 °F
 1620 MPa
@Temperature -79.0 °C
235000 psi
@Temperature -110 °F
Tensile Strength, Yield 1447 MPa
@Strain 0.2 %
209900 psi
@Strain 0.2 %
 1046 MPa
@Strain 0.2 %,
Temperature 345 °C
151700 psi
@Strain 0.2 %,
Temperature 653 °F
 1571 MPa
@Strain 0.2 %,
Temperature -79.0 °C
227900 psi
@Strain 0.2 %,
Temperature -110 °F
Elongation at Break 6.0 %6.0 %in 50 mm
 5.0 %
@Temperature 345 °C
5.0 %
@Temperature 653 °F
in 50 mm
 12 %
@Temperature -79.0 °C
12 %
@Temperature -110 °F
in 50 mm
Modulus of Elasticity 200 GPa29000 ksiTypical for stainless steel
Notched Tensile Strength 1592 MPa230900 psiedge notch root radius of 0.018 mm.
 1065 MPa
@Temperature 345 °C
154500 psi
@Temperature 653 °F
edge notch root radius of 0.018 mm.
 1706 MPa
@Temperature -79.0 °C
247400 psi
@Temperature -110 °F
edge notch root radius of 0.018 mm.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.50 µm/m-°C
@Temperature 21.0 - 93.0 °C
5.28 µin/in-°F
@Temperature 69.8 - 199 °F
 10.6 µm/m-°C
@Temperature 21.0 - 205 °C
5.89 µin/in-°F
@Temperature 69.8 - 401 °F
 11.2 µm/m-°C
@Temperature 21.0 - 315 °C
6.22 µin/in-°F
@Temperature 69.8 - 599 °F
 11.5 µm/m-°C
@Temperature 21.0 - 540 °C
6.39 µin/in-°F
@Temperature 69.8 - 1000 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.75 - 1.5 %0.75 - 1.5 %
Carbon, C <= 0.050 %<= 0.050 %
Chromium, Cr 13.75 - 15 %13.75 - 15 %
Iron, Fe 73 %73 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 2.0 - 3.0 %2.0 - 3.0 %
Nickel, Ni 7.75 - 8.75 %7.75 - 8.75 %
Phosphorus, P <= 0.015 %<= 0.015 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.010 %<= 0.010 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition H1000
Overview of materials for Precipitation Hardening Stainless
17-7 PH Stainless Steel, CH900, plate, sheet, and strip
AISI 1090 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition RH950

MQM14AJ / 13489

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.