(Viewing data as-entered.
Click here
to return)
AISI Type S14800 Stainless Steel condition SRH950, vacuum induction melted
Categories:
Metal
;
Ferrous Metal
;
Stainless Steel
;
Precipitation Hardening Stainless
;
T S10000 Series Stainless Steel
Material Notes:
Specimens were vacuum induction melted, tested in transverse, 25 mm wide, 6.4 mm thick, with an edge notch-root radius of 0.018 mm.
Key Words:
UNS S14800, AMS 5601, AMS 5603; Precipitation Hardening
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Density
7.70
g/cc
In condition SRH950, 7.83 in condition A
Mechanical Properties
Original Value
Comments
Tensile Strength, Ultimate
1502
MPa
1252
MPa
@Temperature 345 °C
1620
MPa
@Temperature -79.0 °C
Tensile Strength, Yield
1447
MPa
@Strain 0.2 %
1046
MPa
@Strain 0.2 %,
Temperature 345 °C
1571
MPa
@Strain 0.2 %,
Temperature -79.0 °C
Elongation at Break
6.0 %
in 50 mm
5.0 %
@Temperature 345 °C
in 50 mm
12 %
@Temperature -79.0 °C
in 50 mm
Modulus of Elasticity
200
GPa
Typical for stainless steel
Notched Tensile Strength
1592
MPa
edge notch root radius of 0.018 mm.
1065
MPa
@Temperature 345 °C
edge notch root radius of 0.018 mm.
1706
MPa
@Temperature -79.0 °C
edge notch root radius of 0.018 mm.
Thermal Properties
Original Value
Comments
CTE, linear
9.50
µm/m-°C
@Temperature 21.0 - 93.0 °C
10.6
µm/m-°C
@Temperature 21.0 - 205 °C
11.2
µm/m-°C
@Temperature 21.0 - 315 °C
11.5
µm/m-°C
@Temperature 21.0 - 540 °C
Component Elements Properties
Original Value
Comments
Aluminum, Al
0.75 - 1.5 %
Carbon, C
<= 0.050 %
Chromium, Cr
13.75 - 15 %
Iron, Fe
73 %
Manganese, Mn
<= 1.0 %
Molybdenum, Mo
2.0 - 3.0 %
Nickel, Ni
7.75 - 8.75 %
Phosphorus, P
<= 0.015 %
Silicon, Si
<= 1.0 %
Sulfur, S
<= 0.010 %
References
for this datasheet.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition H1000
Overview of materials for Precipitation Hardening Stainless
17-7 PH Stainless Steel, CH900, plate, sheet, and strip
AISI 1090 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition RH950
MQM14AJ / 13489
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.