MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Arkema Rilsamid® ASR 20 PA12-CF20
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 12 (PA12); Nylon 12, Carbon Fiber Filled

Material Notes: Property data for dry samples, unless noted.

Information provided by Arkema.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³ISO 1183
Melt Flow 10 g/10 min
@Load 5.00 kg,
Temperature 235 °C
10 g/10 min
@Load 11.0 lb,
Temperature 455 °F
MVR (cm³/10min); ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 128 MPa18600 psiConditioned; ISO 527-1/-2
 132 MPa19100 psiISO 527-1/-2
Elongation at Break 4.0 %4.0 %Conditioned; ISO 527-1/-2
 5.0 %5.0 %ISO 527-1/-2
Tensile Modulus 11.435 GPa1658.5 ksiConditioned; ISO 527-1/-2
 12.58 GPa1825 ksiISO 527-1/-2
Charpy Impact Unnotched  5.80 J/cm²
@Temperature -30.0 °C
27.6 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eU
 5.90 J/cm²
@Temperature 23.0 °C
28.1 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
 5.90 J/cm²
@Temperature -30.0 °C
28.1 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 6.40 J/cm²
@Temperature 23.0 °C
30.5 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eU
Charpy Impact, Notched  1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
Conditioned; ISO 179/1eA
 1.70 J/cm²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
Conditioned; ISO 179/1eA
 1.70 J/cm²
@Temperature 23.0 °C
8.09 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 6.0 ohm-cm6.0 ohm-cmConditioned; IEC 60093
Dielectric Strength 1.00 kV/mm25.4 kV/inConditioned; IEC 60243-1
Comparative Tracking Index 100 V100 VConditioned; IEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 40.0 µm/m-°C22.2 µin/in-°FISO 11359-1/-2
Melting Point 178 °C352 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 175 °C347 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 160 °C320 °FISO 75-1/-2
Vicat Softening Point 170 °C338 °F50°C/h 50N; ISO 306
Flammability, UL94  HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
IEC 60695-11-10
 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
IEC 60695-11-10
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 °C536 °FInjection Molding; ISO 294
Mold Temperature 60.0 °C140 °FInjection Molding; ISO 10724
Hold Pressure 19.0 MPa2760 psiInjection Molding; ISO 294
 
Descriptive Properties
FeaturesAnti-static
 Heat stabilized or stable to heat
 Increased electrical conductivity
 Light stabilized or stable to light
 UV stabilized or stable to weather
FormPellets
Processing MethodsInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
EMS-Grivory Grilamid® L 20 W 20 PA12
EMS-Grivory Grilamid® TR 55 LY PA12/MACMI
Akro-Plastic Akromid® A3 GF 25 1 L black (4672) PA66 + PP, Dry, 25% Glass Filled
Celanese Vectra® C115 Liquid Crystal Polymer (LCP), 15% Glass Reinforced
EMS-Griltech Grilamid® DN 80 Nylon 12 Monofilament

PZARKF863 / 193611

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.