MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Outokumpu 4307 Cr-Ni Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: General purpose steel with good corrosion resistance.

Applications: Wide variety of applications in construction, chemical, petroleum, automobile, and domestic appliance markets.

Available in hot rolled plate (Quarto), hot rolled strip/sheet (CPP), cold rolled strip/sheet, cold rolled narrow strip, bar, and rod forms.

Key Words: EN 1.4307; ASTM 304L; JIS SUS 304L
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.90 g/cc0.285 lb/in³RT
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 165165Outokumpu Typical, 20°C, Hot rolled plate (Quarto); EN 10003-1
 175175Outokumpu Typical, 20°C, Cold rolled strip/sheet; EN 10003-1
Tensile Strength, Ultimate >= 500 MPa>= 72500 psiEN 10002-1
 580 MPa84100 psiOutokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 340 MPa
@Temperature 300 °C
49300 psi
@Temperature 572 °F
EN min.; EN 10002-5
 360 MPa
@Temperature 200 °C
52200 psi
@Temperature 392 °F
EN min.; EN 10002-5
 410 MPa
@Temperature 100 °C
59500 psi
@Temperature 212 °F
EN min.; EN 10002-5
 830 MPa
@Temperature -80.0 °C
120000 psi
@Temperature -112 °F
EN min; EN 10002-5
 1200 MPa
@Temperature -196 °C
174000 psi
@Temperature -321 °F
EN min; EN 10002-5
Tensile Strength, Yield  200 MPa
@Strain 0.2 %
29000 psi
@Strain 0.2 %
EN min., RT; EN 10002-1
 240 MPa
@Strain 1 %
34800 psi
@Strain 1 %
EN min., RT; EN 10002-1
 280 MPa
@Strain 0.2 %
40600 psi
@Strain 0.2 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 320 MPa
@Strain 1 %
46400 psi
@Strain 1 %
Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 81.0 MPa
@Strain 0.2 %,
Temperature 500 °C
11700 psi
@Strain 0.2 %,
Temperature 932 °F
EN min.; EN 10002-5
 89.0 MPa
@Strain 0.2 %,
Temperature 400 °C
12900 psi
@Strain 0.2 %,
Temperature 752 °F
EN min.; EN 10002-5
 100 MPa
@Strain 0.2 %,
Temperature 300 °C
14500 psi
@Strain 0.2 %,
Temperature 572 °F
EN min.; EN 10002-5
 109 MPa
@Strain 1 %,
Temperature 500 °C
15800 psi
@Strain 1 %,
Temperature 932 °F
EN min.; EN 10002-5
 116 MPa
@Strain 1 %,
Temperature 400 °C
16800 psi
@Strain 1 %,
Temperature 752 °F
EN min.; EN 10002-5
 118 MPa
@Strain 0.2 %,
Temperature 200 °C
17100 psi
@Strain 0.2 %,
Temperature 392 °F
EN min.; EN 10002-5
 127 MPa
@Strain 1 %,
Temperature 300 °C
18400 psi
@Strain 1 %,
Temperature 572 °F
EN min.; EN 10002-5
 147 MPa
@Strain 0.2 %,
Temperature 100 °C
21300 psi
@Strain 0.2 %,
Temperature 212 °F
EN min.; EN 10002-5
 147 MPa
@Strain 1 %,
Temperature 200 °C
21300 psi
@Strain 1 %,
Temperature 392 °F
EN min.; EN 10002-5
 181 MPa
@Strain 1 %,
Temperature 100 °C
26300 psi
@Strain 1 %,
Temperature 212 °F
EN min.; EN 10002-5
 220 MPa
@Strain 0.2 %,
Temperature -80.0 °C
31900 psi
@Strain 0.2 %,
Temperature -112 °F
EN min.; EN 10002-5
 290 MPa
@Strain 1 %,
Temperature -80.0 °C
42100 psi
@Strain 1 %,
Temperature -112 °F
EN min.; EN 10002-5
 300 MPa
@Strain 0.2 %,
Temperature -196 °C
43500 psi
@Strain 0.2 %,
Temperature -321 °F
EN min.; EN 10002-5
 400 MPa
@Strain 1 %,
Temperature -196 °C
58000 psi
@Strain 1 %,
Temperature -321 °F
EN min.; EN 10002-5
Elongation at Break >= 45 %>= 45 %EN 10002-1
 55 %55 %Outokumpu Typical, Hot Rolled Plate (Quarto); EN 10002-1
 30 %
@Temperature -196 °C
30 %
@Temperature -321 °F
EN min
 35 %
@Temperature -80.0 °C
35 %
@Temperature -112 °F
EN min
Modulus of Elasticity 200 GPa29000 ksiRT
 165 GPa
@Temperature 500 °C
23900 ksi
@Temperature 932 °F
 172 GPa
@Temperature 400 °C
24900 ksi
@Temperature 752 °F
 179 GPa
@Temperature 300 °C
26000 ksi
@Temperature 572 °F
 186 GPa
@Temperature 200 °C
27000 ksi
@Temperature 392 °F
 194 GPa
@Temperature 100 °C
28100 ksi
@Temperature 212 °F
Poissons Ratio 0.300.30RT
Shear Modulus 77.0 GPa11200 ksicalculated
Impact Test >= 60.0 J>= 44.3 ft-lbHot rolled plate/Cold rolled strip/sheet, 10x10mm test pieces; EN 10045-1
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000730 ohm-cm0.0000730 ohm-cmRT
 
Thermal PropertiesMetricEnglishComments
CTE, linear  16.0 µm/m-°C
@Temperature 100 °C
8.89 µin/in-°F
@Temperature 212 °F
 18.0 µm/m-°C
@Temperature 400 °C
10.0 µin/in-°F
@Temperature 752 °F
Specific Heat Capacity 0.500 J/g-°C0.120 BTU/lb-°FRT
Thermal Conductivity 15.0 W/m-K104 BTU-in/hr-ft²-°FRT
 20.0 W/m-K
@Temperature 400 °C
139 BTU-in/hr-ft²-°F
@Temperature 752 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.020 %0.020 %
Chromium, Cr 18.1 %18.1 %
Iron, Fe 73.58 %73.58 %
Nickel, Ni 8.3 %8.3 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Schmolz + Bickenbach UGIMA 304/304L® Stainless Steel Bar
Industeel CLC 18.9 L General Purpose 18Cr-9Ni Austenitic Stainless Steel
Outokumpu 4404 Cr-Ni-Mo Austenitic Stainless Steel
Outokumpu 4571 Cr-Ni-Mo Austenitic Stainless Steel
Outokumpu 4845 High Temperature Austenitic Stainless Steel

NOUTOK13 / 18728

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.