MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Elastocon TPE Technologies Elastocon® 8150B Thermoplastic Elastomer  (discontinued **)
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Elastocon® 8150B is a black thermoplastic elastomer formulated for applications that require rubber-like properties and a good surface finish. Elastocon® 8150B is well suited for consumer goods and industrial applications requiring U.V. stability. Elastocon® 8150B can be overmolded to polypropylene.

Information provided by Elastocon TPE Technologies, Inc. Elastocon® TPE Technologies has been acquired by Aurora Plastics.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.16 g/cc1.16 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.011 - 0.021 cm/cm0.011 - 0.021 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 4848ASTM D2240
Tensile Strength 5.25 MPa761 psiASTM D412
Elongation at Break 622 %622 %ASTM D412
100% Modulus 2.53 MPa
@Strain 100 %
367 psi
@Strain 100 %
ASTM D412
Compression Set 15 %
@Temperature 20.0 °C,
Time 79200 sec
15 %
@Temperature 68.0 °F,
Time 22.0 hour
ASTM D395B
 
Processing PropertiesMetricEnglishComments
Feed Temperature <= 79.4 °C<= 175 °F
Rear Barrel Temperature 174 - 191 °C345 - 375 °F
Front Barrel Temperature 179 - 196 °C355 - 385 °F
Nozzle Temperature 185 - 204 °C365 - 400 °F
Mold Temperature 21.1 - 37.8 °C70.0 - 100 °F
Back Pressure 0.345 - 0.689 MPa50.0 - 100 psi
 
Descriptive Properties
Injection RateModerate to Fast

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Network Polymers Softflex® 4500
E-Polymers EFLEX® S1040 General
Elastocon TPE Technologies Elastocon® STK40B Thermoplastic Elastomer
Buckeye Polymers BP FLEX A 4812 CU BLK Soft Touch TPE
Barlog Plastics KEBAFLEX SG 35 A.1 TPE-S, Shore A35, natural

PELASC304 / 142480

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.