MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Elektro-Isola G-Etronax EP S Epoxy, Glass Fabric Reinforcement, Green, Sheets
Categories: Polymer; Thermoset; Epoxy; Epoxy, Molded, Glass Fiber Filler

Material Notes: Description: Particularly good electrical and mechanical properties by continuous use, even at high temperatures. Very good chemical resistance. Engineering and insulation material in electrical machinery, transformers and chemical plants. Suitable for mechanical applications. The flexural strength and modulus of elasticity values are measured along the sheet.

Applications: Wear parts/vanes in oil-lubricated vacuum pumps.

Information provided by Elektro-Isola

Key Words: IEC/EN 60893-3-1 EP GC 308, DIN 7735 Hgw 2372.4, NEMA LI 1 G-11
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.90 g/cc
@Temperature 23.0 °C
0.0686 lb/in³
@Temperature 73.4 °F
24h/23°C/50% RH; ISO 1183-A
Water Absorption 0.10 %0.10 %ISO 62-1
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 320 MPa
@Thickness >=1.50 mm
46400 psi
@Thickness >=0.0591 in
24h/23°C/50% RH; ISO 527
Flexural Strength  375 MPa
@Thickness >=1.50 mm,
Temperature 180 °C
54400 psi
@Thickness >=0.0591 in,
Temperature 356 °F
1 hour at temperature/50% RH, Normal to laminate plane; ISO 178
 500 MPa
@Thickness >=1.50 mm,
Temperature 23.0 °C
72500 psi
@Thickness >=0.0591 in,
Temperature 73.4 °F
24h/23°C/50% RH, Normal to laminate plane; ISO 178
Flexural Modulus 24.0 GPa
@Thickness >=1.50 mm
3480 ksi
@Thickness >=0.0591 in
24h/23°C/50% RH, Normal to laminate plane; ISO 178
Compressive Strength 600 MPa
@Thickness >=5.00 mm
87000 psi
@Thickness >=0.197 in
24h/23°C/50% RH, , Normal to laminate plane; ISO 604
Shear Strength 60.0 MPa
@Thickness >=5.00 mm
8700 psi
@Thickness >=0.197 in
Parallel, 24h/23°C/50% RH; IEC 60893-2
Izod Impact, Notched (ISO) 80.0 kJ/m²
@Thickness >=5.00 mm
38.1 ft-lb/in²
@Thickness >=0.197 in
Parallel, 24h/23°C/50% RH; ISO 180/2A
 
Electrical PropertiesMetricEnglishComments
Insulation Resistance 2.00e+8 ohm2.00e+8 ohmafter immersion in water for 24 hr at 23°C; IEC 60167
Dielectric Constant  5.0
@Thickness <=3.00 mm,
Frequency 50 Hz
5.0
@Thickness <=0.118 in,
Frequency 50 Hz
96h/105°C + 1h/23°C/20%RH; IEC 60250
 5.0
@Thickness <=3.00 mm,
Frequency 1e+6 Hz
5.0
@Thickness <=0.118 in,
Frequency 1e+6 Hz
96h/105°C + 1h/23°C/20%RH; IEC 60250
Dielectric Strength  3.15 kV/mm
@Thickness >=3.00 mm,
Temperature 90.0 °C
80.0 kV/in
@Thickness >=0.118 in,
Temperature 194 °F
after 1 hour in oil, Parallel to laminate plane; IEC 60243-1
 18.0 kV/mm
@Thickness 3.00 mm,
Temperature 90.0 °C
457 kV/in
@Thickness 0.118 in,
Temperature 194 °F
after 1 hour in oil, Normal to laminate plane; IEC 60243-1
Dissipation Factor  0.0080
@Thickness <=3.00 mm,
Frequency 50 Hz
0.0080
@Thickness <=0.118 in,
Frequency 50 Hz
96h/105°C + 1h/23°C/20%RH; IEC 60250
 0.010
@Thickness <=3.00 mm,
Frequency 1e+6 Hz
0.010
@Thickness <=0.118 in,
Frequency 1e+6 Hz
96h/105°C + 1h/23°C/20%RH; IEC 60250
Comparative Tracking Index 400 V
@Thickness >=3.00 mm
400 V
@Thickness >=0.118 in
24h/23°C/50% RH; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 200 °C
@Thickness >=3.00 mm,
Time 7.20e+7 sec
392 °F
@Thickness >=0.118 in,
Time 20000 hour
IEC 60216
 
Descriptive Properties
ColorGreen

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Elektro-Isola G-Etronax EP 11 Epoxy, Glass Fabric Reinforcement, Green, Sheets
Elektro-Isola G-Etronax EP FR4 Epoxy, Glass Fabric Reinforcement, Light Yellow, Sheets
Elektro-Isola G-Etronax EP FR Epoxy, Glass Fabric Reinforcement, Light Yellow, Tubes
Norplex-Micarta NP130 Epoxy Glass Laminate Sheet, NEMA FR-4
Elektro-Isola G-Etronax EP 215 S Epoxy, Glass Fabric Reinforcement, Green, Sheets

PELEKT048 / 126924

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.