MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AISI Type S45500 Stainless Steel Strip, annealed at 815°C (1500°F) for 30 minutes, water quenched, strip
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T S40000 Series Stainless Steel

Material Notes: Martensitic, age-hardenable, easily formable (annealed), no corrosion in fresh water, resists staining in normal air atmosphere, good resistance to pitting in 5% salt spray and 5% ferric chloride. For use in service temperatures up to 425°C.

Key Words: UNS S45500, AMS 5578, AMS 5617, AMS 5672, AMS 5860, ASTM A313 (XM-16), ASTM A564 (XM-16), ASTM A705 (XM-16), martensitic, T S45510
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell  311
@Diameter 4.10 mm
311
@Diameter 0.161 in
Converted from Rockwell C hardness.
 318
@Diameter 1.30 mm
318
@Diameter 0.0512 in
Converted from Rockwell C hardness.
Hardness, Knoop  335
@Diameter 4.10 mm
335
@Diameter 0.161 in
Converted from Rockwell C hardness.
 343
@Diameter 1.30 mm
343
@Diameter 0.0512 in
Converted from Rockwell C hardness.
Hardness, Rockwell C  33
@Diameter 4.10 mm
33
@Diameter 0.161 in
 34
@Diameter 1.30 mm
34
@Diameter 0.0512 in
Hardness, Vickers  323
@Diameter 4.10 mm
323
@Diameter 0.161 in
Converted from Rockwell C hardness.
 332
@Diameter 1.30 mm
332
@Diameter 0.0512 in
Converted from Rockwell C hardness.
Tensile Strength, Ultimate  1105 MPa
@Diameter 1.30 mm
160300 psi
@Diameter 0.0512 in
 1105 MPa
@Diameter 4.10 mm
160300 psi
@Diameter 0.161 in
Tensile Strength, Yield  930 MPa
@Strain 0.2 %,
Diameter 4.10 mm
135000 psi
@Strain 0.2 %,
Diameter 0.161 in
 1035 MPa
@Strain 0.2 %,
Diameter 1.30 mm
150100 psi
@Strain 0.2 %,
Diameter 0.0512 in
Elongation at Break  6.0 %
@Diameter 1.30 mm
6.0 %
@Diameter 0.0512 in
in 50 mm
 8.0 %
@Diameter 4.10 mm
8.0 %
@Diameter 0.161 in
in 50 mm
 10 %
@Diameter 1.30 mm
10 %
@Diameter 0.0512 in
in 25 mm.
 18 %
@Diameter 4.10 mm
18 %
@Diameter 0.161 in
in 25 mm.
Modulus of Elasticity 200 GPa29000 ksiTypical for stainless steel
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000900 ohm-cm0.0000900 ohm-cmannealed, 0.000075 Ohm-cm when annealed and aged at 510°C for 4 hours and air cooled.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.6 µm/m-°C
@Temperature 22.0 - 95.0 °C
5.89 µin/in-°F
@Temperature 71.6 - 203 °F
 10.8 µm/m-°C
@Temperature 22.0 - 150 °C
6.00 µin/in-°F
@Temperature 71.6 - 302 °F
 11.2 µm/m-°C
@Temperature 22.0 - 205 °C
6.22 µin/in-°F
@Temperature 71.6 - 401 °F
 11.7 µm/m-°C
@Temperature 22.0 - 260 °C
6.50 µin/in-°F
@Temperature 71.6 - 500 °F
 12.1 µm/m-°C
@Temperature 22.0 - 315 °C
6.72 µin/in-°F
@Temperature 71.6 - 599 °F
Specific Heat Capacity 0.480 J/g-°C0.115 BTU/lb-°FTypical value for stainless steel.
Thermal Conductivity  18.0 W/m-K
@Temperature 100 °C
125 BTU-in/hr-ft²-°F
@Temperature 212 °F
 19.7 W/m-K
@Temperature 200 °C
137 BTU-in/hr-ft²-°F
@Temperature 392 °F
 21.3 W/m-K
@Temperature 300 °C
148 BTU-in/hr-ft²-°F
@Temperature 572 °F
 23.4 W/m-K
@Temperature 400 °C
162 BTU-in/hr-ft²-°F
@Temperature 752 °F
 24.7 W/m-K
@Temperature 500 °C
171 BTU-in/hr-ft²-°F
@Temperature 932 °F
Maximum Service Temperature, Air 425 °C797 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C <= 0.050 %<= 0.050 %
Chromium, Cr 11.8 %11.8 %
Copper, Cu 2.0 %2.0 %
Iron, Fe 73 %73 %
Manganese, Mn <= 0.50 %<= 0.50 %
Molybdenum, Mo <= 0.50 %<= 0.50 %
Nickel, Ni 8.5 %8.5 %
Niobium, Nb (Columbium, Cb) 2.0 %2.0 %
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 0.50 %<= 0.50 %
Sulfur, S <= 0.030 %<= 0.030 %
Titanium, Ti 1.1 %1.1 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Stainless Steel
Carpenter Custom 455® Stainless Steel, Condition H900 (Age Hardened 482°C)
ATI Allvac® Vasco® 455 Specialty Steel, Heat Treatment: 829°C (1525°F) + Age
ASTM A227M Steel Wire, Class I
AISI Type S45500 Stainless Steel, hardened at 815°C (1500°F) for 30 minutes, water quenched, aged at 480°C (900°F) for 4 hours

MQM455K / 13844

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.