Overview of materials for 5000 Series Aluminum Alloy
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "5000 Series Aluminum Alloy". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 0.0160 - 2.84 g/cc0.000579 - 0.103 lb/in³Average value: 1.82 g/cc Grade Count:297
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 28.0 - 18528.0 - 185Average value: 84.9 Grade Count:93
Hardness, Knoop 68.0 - 15068.0 - 150Average value: 98.9 Grade Count:56
Hardness, Rockwell A 35.4 - 46.835.4 - 46.8Average value: 39.2 Grade Count:18
Hardness, Rockwell B 49.0 - 75.049.0 - 75.0Average value: 57.1 Grade Count:21
Hardness, Vickers 46.0 - 13746.0 - 137Average value: 87.6 Grade Count:56
Tensile Strength, Ultimate 110 - 590 MPa16000 - 85600 psiAverage value: 327 MPa Grade Count:115
Tensile Strength, Yield 40.0 - 540 MPa5800 - 78300 psiAverage value: 239 MPa Grade Count:115
Elongation at Break 0.500 - 35.0 %0.500 - 35.0 %Average value: 11.9 % Grade Count:114
Modulus of Elasticity 68.9 - 73.0 GPa10000 - 10600 ksiAverage value: 70.3 GPa Grade Count:104
Compressive Yield Strength 0.138 - 325 MPa20.0 - 47100 psiAverage value: 15.9 MPa Grade Count:104
Compressive Modulus 0.0689 - 74.0 GPa10.0 - 10700 ksiAverage value: 13.4 GPa Grade Count:117
Notched Tensile Strength 207 - 331 MPa30000 - 48000 psiAverage value: 263 MPa Grade Count:8
Ultimate Bearing Strength 248 - 669 MPa36000 - 97000 psiAverage value: 492 MPa Grade Count:18
Bearing Yield Strength 83.0 - 476 MPa12000 - 69000 psiAverage value: 280 MPa Grade Count:18
Poissons Ratio 0.330 - 0.3600.330 - 0.360Average value: 0.331 Grade Count:86
Fatigue Strength 82.7 - 365 MPa12000 - 52900 psiAverage value: 150 MPa Grade Count:41
Fracture Toughness 35.0 - 185 MPa-m½31.9 - 168 ksi-in½Average value: 117 MPa-m½ Grade Count:4
Machinability 10.0 - 50.0 %10.0 - 50.0 %Average value: 34.0 % Grade Count:25
Shear Modulus 0.0469 - 72.4 GPa6.80 - 10500 ksiAverage value: 8.44 GPa Grade Count:179
Shear Strength 0.138 - 270 MPa20.0 - 39200 psiAverage value: 31.1 MPa Grade Count:187
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000316 - 0.00000660 ohm-cm0.00000316 - 0.00000660 ohm-cmAverage value: 0.00000503 ohm-cm Grade Count:98
 
Thermal PropertiesMetricEnglishComments
CTE, linear 21.8 - 26.1 µm/m-°C12.1 - 14.5 µin/in-°FAverage value: 24.2 µm/m-°C Grade Count:102
Specific Heat Capacity 0.857 - 0.960 J/g-°C0.205 - 0.229 BTU/lb-°FAverage value: 0.897 J/g-°C Grade Count:86
Thermal Conductivity 105 - 205 W/m-K729 - 1420 BTU-in/hr-ft²-°FAverage value: 141 W/m-K Grade Count:102
Melting Point 568 - 657 °C1060 - 1220 °FAverage value: 623 °C Grade Count:82
Solidus 568 - 638 °C1060 - 1180 °FAverage value: 601 °C Grade Count:82
Liquidus 635 - 657 °C1180 - 1220 °FAverage value: 646 °C Grade Count:82
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 343 - 413 °C650 - 775 °FAverage value: 351 °C Grade Count:83
Hot-Working Temperature 260 - 510 °C500 - 950 °FAverage value: 387 °C Grade Count:83
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 88.2 - 99.8 %88.2 - 99.8 %Average value: 95.5 % Grade Count:190
Beryllium, Be 0.000500 - 0.000800 %0.000500 - 0.000800 %Average value: 0.000704 % Grade Count:28
Chromium, Cr 0.0100 - 0.500 %0.0100 - 0.500 %Average value: 0.175 % Grade Count:163
Copper, Cu 0.0300 - 0.800 %0.0300 - 0.800 %Average value: 0.145 % Grade Count:182
Cr + Mn 0.100 - 0.700 %0.100 - 0.700 %Average value: 0.377 % Grade Count:10
Gallium, Ga 0.0300 - 0.0500 %0.0300 - 0.0500 %Average value: 0.0340 % Grade Count:5
Iron, Fe 0.00800 - 1.20 %0.00800 - 1.20 %Average value: 0.424 % Grade Count:174
Lead, Pb 0.00300 - 1.80 %0.00300 - 1.80 %Average value: 0.534 % Grade Count:3
Magnesium, Mg 0.200 - 6.20 %0.200 - 6.20 %Average value: 3.15 % Grade Count:190
Manganese, Mn 0.0100 - 1.80 %0.0100 - 1.80 %Average value: 0.410 % Grade Count:188
Nickel, Ni 0.0100 - 0.100 %0.0100 - 0.100 %Average value: 0.0440 % Grade Count:5
Scandium, Sc 0.0500 - 0.550 %0.0500 - 0.550 %Average value: 0.267 % Grade Count:3
Si+Fe 0.350 - 0.450 %0.350 - 0.450 %Average value: 0.422 % Grade Count:16
Silicon, Si 0.0100 - 1.40 %0.0100 - 1.40 %Average value: 0.302 % Grade Count:174
Titanium, Ti 0.00800 - 0.200 %0.00800 - 0.200 %Average value: 0.135 % Grade Count:130
Vanadium, V 0.0500 %0.0500 %Average value: 0.0500 % Grade Count:14
Zinc, Zn 0.0100 - 2.80 %0.0100 - 2.80 %Average value: 0.260 % Grade Count:184
Zirconium, Zr 0.0500 - 0.300 %0.0500 - 0.300 %Average value: 0.158 % Grade Count:26
Zr+Ti 0.150 %0.150 %Average value: 0.150 % Grade Count:8

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.