Commercial Fine Gold, Cast
Categories: Metal; Nonferrous Metal; Precious Metal; Gold Alloy; Pure Element

Material Notes: Usual purity is 99.95-99.98%. Called proof gold if over 99.99% pure.

Key Words: Gold, Au
Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 19.32 g/cc0.6980 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 3333
Tensile Strength, Ultimate 125 MPa18100 psi
Elongation at Break 30 %30 %
Modulus of Elasticity 74.5 GPa10800 ksi
Poissons Ratio 0.420.42
Fatigue Strength 31.7 MPa
@# of Cycles 1.00e+7
4600 psi
@# of Cycles 1.00e+7
reverse bend
Shear Modulus 26.2 GPa3800 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000235 ohm-cm0.00000235 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 66.2 J/g28.5 BTU/lb
CTE, linear  14.2 µm/m-°C
@Temperature 20.0 °C
7.89 µin/in-°F
@Temperature 68.0 °F
 14.6 µm/m-°C
@Temperature 250 °C
8.11 µin/in-°F
@Temperature 482 °F
 15.2 µm/m-°C
@Temperature 500 °C
8.44 µin/in-°F
@Temperature 932 °F
 16.7 µm/m-°C
@Temperature 950 °C
9.28 µin/in-°F
@Temperature 1740 °F
Specific Heat Capacity 0.130 J/g-°C0.0311 BTU/lb-°F
Thermal Conductivity 300 W/m-K
@Temperature 0.000 °C
2080 BTU-in/hr-ft²-°F
@Temperature 32.0 °F
Melting Point 1064 °C1947 °F
 
Optical PropertiesMetricEnglishComments
Emissivity (0-1) 0.040
@Temperature 100 °C
0.040
@Temperature 212 °F
total spectrum
Reflection Coefficient, Visible (0-1) 0.850.85600 nm
 
Processing PropertiesMetricEnglishComments
Casting Temperature 1095 - 1300 °C2003 - 2370 °F
 
Component Elements PropertiesMetricEnglishComments
Gold, Au >= 99.95 %>= 99.95 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.