MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Nilit Nilamid A3 H6 G5 25% Glass Reinforced PA66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 30% Glass Fiber Filled

Material Notes: Description: Nilamid A3 H6 G5 is a 25% glass fiber reinforced NYLON 66 with a special stabilization system against hot oil and grease. As a result of this stabilization, the material has a brown natural color. It is used for applications which run in hot mineral oil, such as bearing cages, cam shafts and couplings. Because this material also demonstrates good hot air heat stability and has a low ionic content, it is also used for electrical applications such as bobbins.

Key characteristics:

  • Excellent heat stability and stability against hot oil and grease
  • Good overall mechanical performance up to 150°C
  • Brown natural color
  • Easy processing

Information provided by NILIT.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.32 g/cc0.0477 lb/in³ASTM D792, ISO 1183
Water Absorption 0.80 %0.80 %23°C, 24h in H2O; sim. ISO 62
Water Absorption at Saturation 5.5 %5.5 %sim. ISO 62
Linear Mold Shrinkage, Flow 0.0035 cm/cm0.0035 in/inEuronil
Linear Mold Shrinkage, Transverse 0.0055 cm/cm0.0055 in/inEuronil
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 150 MPa21800 psiISO 527, ASTM D638
Elongation at Break 3.0 %3.0 %ISO 527, ASTM D638
Flexural Yield Strength 230 MPa33400 psiISO 178, ASTM D790
Flexural Modulus 7.80 GPa1130 ksiISO 178, ASTM D790
 4.50 GPa
@Temperature 90.0 °C
653 ksi
@Temperature 194 °F
ISO 178, ASTM D790
Izod Impact, Notched (ISO) 8.00 kJ/m²
@Temperature 23.0 °C
3.81 ft-lb/in²
@Temperature 73.4 °F
ISO 180/1A
Charpy Impact Unnotched 4.80 J/cm²22.8 ft-lb/in²ISO 179
Charpy Impact, Notched 0.900 J/cm²4.28 ft-lb/in²ISO 179
 
Electrical PropertiesMetricEnglishComments
Dielectric Strength 20.0 kV/mm
@Thickness 2.00 mm
508 kV/in
@Thickness 0.0787 in
ASTM D149
Comparative Tracking Index  350 V
@Thickness 3.20 mm
350 V
@Thickness 0.126 in
Sol. B; IEC 112, UL 746A
 500 V
@Thickness 3.20 mm
500 V
@Thickness 0.126 in
Sol. A; IEC 112, UL 746A
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 130 °C266 °F20,000 hr; IEC 216
Deflection Temperature at 0.46 MPa (66 psi) 255 °C491 °FISO 75, ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 248 °C478 °FISO 75, ASTM D648
Vicat Softening Point 250 °C482 °F49 N; ISO 306, ASTM D1525
 255 °C491 °F9.8 N; ISO 306, ASTM D1525
Flammability, UL94  HB
@Thickness 0.800 mm
HB
@Thickness 0.0315 in
 HB
@Thickness 3.20 mm
HB
@Thickness 0.126 in
Oxygen Index 24 %24 %ASTM D2863
Glow Wire Flammability Index  650 °C
@Thickness 0.800 mm
1200 °F
@Thickness 0.0315 in
IEC 694-2-12
 650 °C
@Thickness 3.20 mm
1200 °F
@Thickness 0.126 in
IEC 694-2-12
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 280 - 295 °C536 - 563 °F
Zone 1 270 - 290 °C518 - 554 °Fhopper
Zone 2 275 - 290 °C527 - 554 °F
Zone 3 280 - 295 °C536 - 563 °F
Zone 4 280 - 295 °C536 - 563 °F
Melt Temperature 275 - 300 °C527 - 572 °FDo not melt above 300°C
Mold Temperature 90.0 - 110 °C194 - 230 °FPreferred
Drying Temperature 80.0 - 85.0 °C176 - 185 °F
Dry Time 4 hour4 hour
Injection Pressure 70.0 - 100 MPa10200 - 14500 psi
 
Descriptive Properties
Clamping Forcein tons, 0.7 times the projected surface area in cm2
Heat Resistance - Ball TestOKat 125°C, IEC 309
 OKat 165°C, IEC 309
Holding Pressure90 Mpa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, 30% Glass Fiber Filled
Avient Bergamid™ A70 G30 U Polyamide 66 (Nylon 66)
LATI Kelon® B FR H2 CEG/500-V0CT3 PA 6, Glass/Mineral Reinforced, Flame Retardant, Heat Stabilized
LATI Later 4 G/30-V0 PBT, 30% Glass Fiber Reinforced, Flame Retardant
LATI Laticonther 62 CEG/500-V0HF1 PA 6, Glass/Mineral Reinforced, Flame Retardant

PLBN29 / 50418

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.