MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

SABIC LEXAN™ Copolymer HFD1830 Polycarbonate (PC) (Asia)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: 40 MFR LEXAN High Flow Ductile Copolymer UV Stabilized

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.20 g/cc1.20 g/ccASTM D792
Density 1.20 g/cc0.0434 lb/in³ASTM D792
 1.20 g/cc0.0434 lb/in³ISO 1183
Moisture Absorption 0.150 %0.150 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.30 %0.30 %ISO 62-1
Viscosity 38 cP
@Load 1.20 kg,
Temperature 300 °C
38 cP
@Load 2.65 lb,
Temperature 572 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 40 g/10 min
@Load 1.20 kg,
Temperature 300 °C
40 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 120120ASTM D785
Tensile Strength at Break 56.0 MPa8120 psi50 mm/min; ASTM D638
 56.0 MPa8120 psi50 mm/min; ISO 527
Tensile Strength, Yield 60.0 MPa8700 psi50 mm/min; ASTM D638
 63.0 MPa9140 psi50 mm/min; ISO 527
Elongation at Break 97 %97 %50 mm/min; ISO 527
 130 %130 %50 mm/min; ASTM D638
Elongation at Yield 5.5 %5.5 %50 mm/min; ASTM D638
 6.0 %6.0 %50 mm/min; ISO 527
Tensile Modulus 2.18 GPa316 ksi1 mm/min; ISO 527
 2.27 GPa329 ksi5 mm/min; ASTM D638
Flexural Strength 91.0 MPa13200 psiyield, 2 mm/min; ISO 178
 100 MPa14500 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2.18 GPa316 ksi2 mm/min; ISO 178
 2.24 GPa325 ksi1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 728 J537 ft-lbASTM D256
 115 J
@Temperature -30.0 °C
84.8 ft-lb
@Temperature -22.0 °F
ASTM D256
 699 J
@Temperature 0.000 °C
516 ft-lb
@Temperature 32.0 °F
ASTM D256
Izod Impact, Notched (ISO) 58.0 kJ/m²27.6 ft-lb/in²80*10*3; ISO 180/1A
 11.0 kJ/m²
@Temperature -30.0 °C
5.23 ft-lb/in²
@Temperature -22.0 °F
80*10*3; ISO 180/1A
Izod Impact, Unnotched (ISO) NBNB80*10*3; ISO 180/1U
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
80*10*3; ISO 180/1U
Charpy Impact Unnotched NBNBEdgew 80*10*3 sp=62mm; ISO 179/1eU
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 6.40 J/cm²30.5 ft-lb/in²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 1.30 J/cm²
@Temperature -30.0 °C
6.19 ft-lb/in²
@Temperature -22.0 °F
Edgew 80*10*3 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 56.0 J41.3 ft-lbASTM D3763
Impact Test 95.0 J70.1 ft-lbMultiaxial Impact; ISO 6603
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  80.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
44.4 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 80.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
44.4 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
CTE, linear, Transverse to Flow  80.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
44.4 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 80.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
44.4 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Hot Ball Pressure Test 125 °C257 °FPASS; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 121 °C
@Thickness 3.20 mm
250 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 115 °C239 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 110 °C
@Thickness 3.20 mm
230 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 129 °C264 °FRate B/50; ISO 306
 130 °C266 °FRate B/120; ISO 306
 135 °C275 °FRate B/50; ASTM D1525
UL RTI, Electrical 105 °C221 °FUL 746B
UL RTI, Mechanical with Impact 105 °C221 °FUL 746B
UL RTI, Mechanical without Impact 105 °C221 °FUL 746B
Flammability, UL94  HB
@Thickness >=0.500 mm
HB
@Thickness >=0.0197 in
UL 94
 V-2
@Thickness >=1.00 mm
V-2
@Thickness >=0.0394 in
UL 94
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5821.582ASTM D542
Haze <= 1.0 %
@Thickness 2.54 mm
<= 1.0 %
@Thickness 0.100 in
ASTM D1003
Transmission, Visible 88 %
@Thickness 2.54 mm
88 %
@Thickness 0.100 in
ASTM D1003
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 255 - 300 °C491 - 572 °F
Zone 2 250 - 295 °C482 - 563 °F
Zone 3 260 - 305 °C500 - 581 °F
Melt Temperature 260 - 305 °C500 - 581 °FInjection Molding
Mold Temperature 50.0 - 80.0 °C122 - 176 °F
Drying Temperature 105 - 110 °C221 - 230 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 24.0 hour24.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 40 - 60 %40 - 60 %
Vent Depth 0.00380 - 0.00760 cm0.00150 - 0.00299 in
Screw Speed 35 - 75 rpm35 - 75 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH80326 / 288273

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.