MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
ITW Devcon® Tru-Bond™ PB 3500 Coating
Categories: Polymer; Thermoset

Material Notes: The Tru-Bond™ Plastic Bonding (PB) Series of products provide UV/Visible light cured bonds to a wide range of plastics including ABS, polycarbonate, PET, PETG, flexible vinyl, urethanes and acrylics. The adhesive creates a flexible resilient polymer with outstanding impact resistance and flex. These products can also cure through most translucent substrates and UV blocked plastics.

Information provided by ITW Performance Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.00 g/ccCured
Volatile Organic Compounds (VOC) Content <= 1.0 g/lUncured
Water Absorption 5.0 %
@Time 86400 sec
cured; ASTM D570
Brookfield Viscosity 3500 cPBrookfield RV Spindle 3, 6rpm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 50
Tensile Strength 480 psiASTM D882
Elongation at Break 325 %ASTM D882
Modulus of Elasticity 0.00400 GPacured
Adhesive Bond Strength 572 psiLap Shear; PETG
 613 psiLap Shear; Acrylic
 968 psiLap Shear; Polycarbonate
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 300 °F
Minimum Service Temperature, Air -65.0 °F
Flash Point >= 171 °F
Shrinkage 2.1 %Linear
 9.0 %Volume
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.50cured; ASTM D542
Transmission, Visible >= 98 %cured
 
Processing PropertiesOriginal ValueComments
Shelf Life 24.0 Month
 
Descriptive Properties
Boiling Water (%)2.6Cured. 2 hrs. ASTM D570
Colorclearcured
 Clear liquidUncured
Solubilityketones, oxygenated solventsUncured
ViscosityLow

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PITWD9225 / 239734

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.