MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
8% Aluminum Bronze, UNS C61000
Categories: Metal; Nonferrous Metal; Copper Alloy; Bronze

Material Notes: Good to excellent corrosion resistance. Good hot and cold workability.

Applications: bolts, pump parts, shafts, tie rods, overlay on steel for wearing surfaces.

Properties typical for rod, 25mm in diameter.

Key Words: CDA 610
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.78 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 60O60 temper
 85H04 temper
Tensile Strength, Ultimate 480 MPaO60 temper
 550 MPaH04 temper
Tensile Strength, Yield 205 MPaO60 temper
 380 MPaH04 temper
Elongation at Break 25 %in 50 mm, H04 temper
 65 %in 50 mm, O60 temper
Modulus of Elasticity 117 GPa
Poissons Ratio 0.33Calculated
Machinability 20 %UNS C36000 (free-cutting brass) = 100%
Forgeability 70 %
Shear Modulus 44.0 GPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000115 ohm-cm
@Temperature 20.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 17.9 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.375 J/g-°C
Thermal Conductivity 69.0 W/m-K
@Temperature 20.0 °C
Melting Point <= 1040 °C
Liquidus 1040 °C
Annealing Point 1100 - 1250 °F
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 600 - 675 °C
Hot-Working Temperature 760 - 875 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 6.0 - 8.5 %
Copper, Cu 92 %
Iron, Fe <= 0.50 %
Lead, Pb <= 0.020 %
Other, total <= 0.50 %
Silicon, Si <= 0.10 %
Zinc, Zn <= 0.20 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum Bronze, UNS C61300, Annealed
Nickel Aluminum Bronze, UNS C63000, HR50 Temper
Aluminum bronze 5%, UNS C60800
Aluminum Bronze D, UNS C61400, Annealed Rod
Aluminum Bronze, UNS C61300, Cold Finished

MC61000b1 / 11578

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.