Physical Properties | Original Value | Comments |
---|
Density | 7.10 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Vickers | 230 @Diameter 4.00 mm |
Tensile Strength, Ultimate | 9.00 MPa @Temperature 1300 °C |
| 12.0 MPa @Temperature 1200 °C |
| 16.0 MPa @Temperature 1100 °C |
| 23.0 MPa @Temperature 1000 °C |
| 40.0 MPa @Temperature 900 °C |
| 680 MPa @Thickness 4.00 mm |
Tensile Strength, Yield | 470 MPa @Strain 0.2 %, Thickness 4.00 mm |
Elongation at Break | 20 % @Thickness 4.00 mm |
Creep Strength | 0.400 MPa @Temperature 1400 °C |
| 0.700 MPa @Temperature 1300 °C |
| 1.20 MPa @Temperature 1200 °C |
| 2.30 MPa @Temperature 1100 °C |
| 3.50 MPa @Temperature 900 °C |
| 8.20 MPa @Temperature 800 °C |
Rupture Strength | 0.200 MPa @Temperature 1400 °C, Time 3.60e+7 sec |
| 0.500 MPa @Temperature 1400 °C, Time 3.60e+6 sec |
| 0.700 MPa @Temperature 1200 °C, Time 3.60e+7 sec |
| 1.30 MPa @Temperature 1400 °C, Time 360000 sec |
| 1.60 MPa @Temperature 1200 °C, Time 3.60e+6 sec |
| 2.20 MPa @Temperature 1000 °C, Time 3.60e+7 sec |
| 3.30 MPa @Temperature 1200 °C, Time 360000 sec |
| 3.40 MPa @Temperature 1000 °C, Time 3.60e+6 sec |
| 8.20 MPa @Temperature 800 °C, Time 3.60e+7 sec |
| 11.3 MPa @Temperature 800 °C, Time 3.60e+6 sec |
| 15.0 MPa @Temperature 800 °C, Time 360000 sec |
Modulus of Elasticity | 130 GPa @Temperature 1000 °C |
| 150 GPa @Temperature 800 °C |
| 170 GPa @Temperature 600 °C |
| 190 GPa @Temperature 400 °C |
| 205 GPa @Temperature 200 °C |
| 210 GPa @Temperature 100 °C |
| 220 GPa @Temperature 20.0 °C |
Poissons Ratio | 0.30 |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 0.000145 ohm-cm |
| 0.0000100 ohm-cm @Temperature 100 - 400 °C |
| 0.0000101 ohm-cm @Temperature 500 °C |
| 0.0000102 ohm-cm @Temperature 600 - 700 °C |
| 0.0000103 ohm-cm @Temperature 800 - 900 °C |
| 0.0000104 ohm-cm @Temperature 1000 - 1300 °C |
| 0.0000105 ohm-cm @Temperature 1400 °C |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 11.0 µm/m-°C @Temperature 20.0 - 250 °C |
| 12.0 µm/m-°C @Temperature 20.0 - 500 °C |
| 14.0 µm/m-°C @Temperature 20.0 - 750 °C |
| 15.0 µm/m-°C @Temperature 20.0 - 1000 °C |
| 16.0 µm/m-°C @Temperature 20.0 - 1200 °C |
| 16.0 µm/m-°C @Temperature 20.0 - 1400 °C |
Specific Heat Capacity | 0.460 J/g-°C @Temperature 20.0 °C |
| 0.560 J/g-°C @Temperature 200 °C |
| 0.630 J/g-°C @Temperature 400 °C |
| 0.710 J/g-°C @Temperature 800 °C |
| 0.720 J/g-°C @Temperature 1000 °C |
| 0.740 J/g-°C @Temperature 1200 °C |
| 0.750 J/g-°C @Temperature 600 °C |
| 0.800 J/g-°C @Temperature 1400 °C |
Thermal Conductivity | 11.0 W/m-K @Temperature 50.0 °C |
| 20.0 W/m-K @Temperature 600 °C |
| 22.0 W/m-K @Temperature 800 °C |
| 26.0 W/m-K @Temperature 1000 °C |
| 27.0 W/m-K @Temperature 1200 °C |
| 35.0 W/m-K @Temperature 1400 °C |
Melting Point | 1500 °C |
Maximum Service Temperature, Air | 1425 °C |
|
Optical Properties | Original Value | Comments |
---|
Emissivity (0-1) | 0.70 |
|
Component Elements Properties | Original Value | Comments |
---|
Aluminum, Al | 5.0 % |
Carbon, C | 0.080 % |
Chromium, Cr | 20.5 - 23.5 % |
Iron, Fe | 68.42 - 70.32 % |
Manganese, Mn | >= 0.40 % |
Molybdenum, Mo | 3.0 % |
Silicon, Si | >= 0.70 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.