MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

Henkel Loctite® IND405™ HDT50 High Elongation Clear Resin for 3D Printing
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer

Material Notes: LOCTITE® 3D IND405™ is a high elongation and high toughness material with outstanding impact resistance and excellent surface finish. This stiff and durable high performance material is ideal for a wide variety of tools in the production floor, including manufacturing aids and final parts such as housings and consumer goods applications. The unique set of performance attributes makes it comparable to an unfilled thermoplastic like polypropylene. Parts can be machined, tapped, or polished for final finish.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³Liquid; ASTM D1475
 1.126 g/cc0.04068 lb/in³Green; ASTM D1475
 1.34 g/cc0.0484 lb/in³Post Process; ASTM D1475
Water Absorption  0.99 %
@Time 86400 sec
0.99 %
@Time 24.0 hour
Post Process Dymax 5 min/per side; ASTM 570
 1.2 %
@Time 86400 sec
1.2 %
@Time 24.0 hour
Post Process UV Cube 15 min/per side; ASTM 570
Viscosity 2300 cP2300 cPASTM D7867
ASTM Color -1.205-1.205a* Green / no post-processing; ASTM E308
 -0.650-0.650a*, 0 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 -0.520-0.520a* Dymax 5000EC 5 minutes / side; ASTM E308
 -0.470-0.470a*, 240 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 -0.320-0.320a* Loctite CL36 60 min/side [9; ASTM E308
 0.470.47dE, 240 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 0.890.89b* Loctite CL36 60 min/side [9; ASTM E308
 0.940.94C* Loctite CL36 60 min/side [9; ASTM E308
 1.031.03b*, 0 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 1.171.17dE Dymax 5000EC 5 minutes / side; ASTM E308
 1.221.22C*, 0 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 1.2651.265b* Dymax 5000EC 5 minutes / side; ASTM E308
 1.371.37C* Dymax 5000EC 5 minutes / side; ASTM E308
 1.421.42b*, 240 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 1.491.49C*, 240 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 1.831371.83137dE Loctite CL36 60 min/side [9; ASTM E308
 2.1952.195b* Green / no post-processing; ASTM E308
 2.52.5C* Green / no post-processing; ASTM E308
 90.8690.86L*, 0 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 91.0691.06L*, 240 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 92.1892.18L* Loctite CL36 60 min/side [9; ASTM E308
 92.25592.255L* Dymax 5000EC 5 minutes / side; ASTM E308
 92.42592.425L* Green / no post-processing; ASTM E308
 108.47108.47h, 240 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 109.88109.88h Loctite CL36 60 min/side [9; ASTM E308
 112.28112.28h Dymax 5000EC 5 minutes / side; ASTM E308
 118.735118.735h Green / no post-processing; ASTM E308
 122.49122.49h, 0 hrs, QUV exterior weathering conditions; ASTM G-154—Cycle 1 & ASTM E308
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D  70
@Time 10800 sec
70
@Time 3.00 hour
Post Process UV Cube 15 min/per side; ASTM D2240
 74
@Time 0.000 sec
74
@Time 0.000 hour
Post Process UV Cube 15 min/per side; ASTM D2240
 78
@Time 0.000 sec
78
@Time 0.000 hour
Post Process Dymax 5 min/per side; ASTM D2240
 80
@Time 10800 sec
80
@Time 3.00 hour
Post Process Dymax 5 min/per side; ASTM D2240
Tensile Strength at Break 27.0 - 33.0 MPa3920 - 4790 psiGreen; ASTM D638
 33.0 - 37.0 MPa4790 - 5370 psiPost Process UV Cube 15 min/per side; ASTM D638
 38.0 - 46.0 MPa5510 - 6670 psiPost Process Dymax 5 min/per side; ASTM D638
 6.20 MPa
@Temperature 100 °C
899 psi
@Temperature 212 °F
Post-processed; ASTM D638
 52.0 MPa
@Temperature 40.0 °C
7540 psi
@Temperature 104 °F
Post-processed; ASTM D638
 114 MPa
@Temperature -40.0 °C
16500 psi
@Temperature -40.0 °F
Post-processed; ASTM D638
 37.0 - 39.0 MPa
@Time 2.88e+6 sec
5370 - 5660 psi
@Time 800 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 38.0 - 43.0 MPa
@Time 1.87e+6 sec
5510 - 6240 psi
@Time 520 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 38.0 - 44.0 MPa
@Time 1.08e+6 sec
5510 - 6380 psi
@Time 300 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 46.0 - 52.0 MPa
@Time 0.000 sec
6670 - 7540 psi
@Time 0.000 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
Tensile Strength, Yield 17.0 - 19.0 MPa2470 - 2760 psiGreen; ASTM D638
 35.0 - 37.0 MPa5080 - 5370 psiPost Process UV Cube 15 min/per side; ASTM D638
 42.0 - 44.0 MPa6090 - 6380 psiPost Process Dymax 5 min/per side; ASTM D638
 20.0 MPa
@Temperature 40.0 °C
2900 psi
@Temperature 104 °F
Post-processed; ASTM D638
 74.0 MPa
@Temperature -40.0 °C
10700 psi
@Temperature -40.0 °F
Post-processed; ASTM D638
 39.0 - 41.0 MPa
@Time 1.08e+6 sec
5660 - 5950 psi
@Time 300 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 41.0 - 43.0 MPa
@Time 0.000 sec
5950 - 6240 psi
@Time 0.000 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 43.0 - 45.0 MPa
@Time 1.87e+6 sec
6240 - 6530 psi
@Time 520 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 44.0 - 46.0 MPa
@Time 2.88e+6 sec
6380 - 6670 psi
@Time 800 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
Elongation at Break 106 - 134 %106 - 134 %Green; ASTM D638
 112 - 128 %112 - 128 %Post Process Dymax 5 min/per side; ASTM D638
 114 - 146 %114 - 146 %Post Process UV Cube 15 min/per side; ASTM D638
 12.0 %
@Temperature -40.0 °C
12.0 %
@Temperature -40.0 °F
Post-processed; ASTM D638
 95.0 %
@Temperature 100 °C
95.0 %
@Temperature 212 °F
Post-processed; ASTM D638
 140 %
@Temperature 40.0 °C
140 %
@Temperature 104 °F
Post-processed; ASTM D638
 30 - 62 %
@Time 2.88e+6 sec
30 - 62 %
@Time 800 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 47 - 79 %
@Time 1.87e+6 sec
47 - 79 %
@Time 520 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 66 - 90 %
@Time 1.08e+6 sec
66 - 90 %
@Time 300 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 104 - 128 %
@Time 0.000 sec
104 - 128 %
@Time 0.000 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
Modulus of Elasticity 0.774 - 0.826 GPa112 - 120 ksiGreen; ASTM D638
 1.267 - 1.333 GPa183.8 - 193.3 ksiPost Process UV Cube 15 min/per side; ASTM D638
 1.469 - 1.531 GPa213.1 - 222.1 ksiPost Process Dymax 5 min/per side; ASTM D638
 0.300 GPa
@Temperature 60.0 °C
43.5 ksi
@Temperature 140 °F
Post-processed; ASTM D638
 0.690 GPa
@Temperature 40.0 °C
100 ksi
@Temperature 104 °F
Post-processed; ASTM D638
 2.20 GPa
@Temperature -40.0 °C
319 ksi
@Temperature -40.0 °F
Post-processed; ASTM D638
 1.24 - 1.446 GPa
@Time 1.08e+6 sec
180 - 209.7 ksi
@Time 300 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 1.352 - 1.472 GPa
@Time 0.000 sec
196.1 - 213.5 ksi
@Time 0.000 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 1.434 - 1.504 GPa
@Time 1.87e+6 sec
208.0 - 218.1 ksi
@Time 520 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
 1.427 - 1.529 GPa
@Time 2.88e+6 sec
207.0 - 221.8 ksi
@Time 800 hour
QUV exterior weathering conditions; ASTM G-154—Cycle 1
Izod Impact, Notched 0.500 J/cm0.937 ft-lb/inPost Process UV Cube 15 min/per side; ASTM D256
 0.500 J/cm0.937 ft-lb/inPost Process Dymax 5 min/per side; ASTM D256
 0.700 - 0.740 J/cm1.31 - 1.39 ft-lb/inASTM D256
Izod Impact, Unnotched >= 15.0 J/cm>= 28.1 ft-lb/inPost Process UV Cube 15 min/per side; ASTM D256
 >= 15.0 J/cm>= 28.1 ft-lb/inPost Process Dymax 5 min/per side; ASTM D256
Abrasion 5050[mg], Taber, Post Process Dymax 5 min/per side; ASTM D4060-19
 9090[mg], Taber, Post Process UV Cube 15 min/per side; ASTM D4060-19
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 8.55e+14 ohm-cm8.55e+14 ohm-cmASTM D257
Surface Resistance 1.24e+15 ohm1.24e+15 ohmASTM D257
Dielectric Constant  3.80
@Frequency 1e+6 Hz
3.80
@Frequency 1e+6 Hz
AC, XY; ASTM D150
 4.20
@Frequency 1000 Hz
4.20
@Frequency 1000 Hz
AC, XY; ASTM D150
 4.40
@Frequency 50 Hz
4.40
@Frequency 50 Hz
AC, XY; ASTM D150
Dielectric Strength 27.4 kV/mm696 kV/inASTM D149
Dissipation Factor  0.0170
@Frequency 1000 Hz
0.0170
@Frequency 1000 Hz
AC, XY; ASTM D150
 0.0250
@Frequency 50 Hz
0.0250
@Frequency 50 Hz
AC, XY; ASTM D150
 0.428
@Frequency 1e+6 Hz
0.428
@Frequency 1e+6 Hz
AC, XY; ASTM D150
 
Thermal PropertiesMetricEnglishComments
CTE, linear 91.14 µm/m-°C
@Temperature -30.0 - 45.0 °C
50.63 µin/in-°F
@Temperature -22.0 - 113 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 53.0 °C127 °FPost Process UV Cube 15 min/per side; ASTM D648
 53.0 °C127 °FPost Process Dymax 5 min/per side; ASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PLOCT00_a / 280637

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.