MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Versalis Greenflex® FD 23 Ethylene Vinyl Acetate Copolymer - Blown Film Extrusion
Categories: Polymer; Film; Thermoplastic; Ethylene Vinyl Acetate; Ethylene Vinyl Acetate Copolymer (EVA), Film Grade

Material Notes: Greenflex FD 23 is an ethylene vinyl acetate copolymer (EVA) suitable for blown film extrusion. Greenflex FD 23 is a version of Greenflex FD 20 with added slip and antiblocking agents.

Films produced with Greenflex FD 23 exhibit good optical properties, high impact resistance, tensile strength, elongation at break and low creep.

Main Applications: Greenflex FD 23 is recommended for thermo-shrinkable films for food packaging, including deep-frozen food packaging.

Information provided by Polimeri Europa.

Versalis is the Eni subsidiary containing the plastics and rubber businesses.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.924 g/ccISO 1183
Vinyl Acetate Content 5.0 %Internal Method
Thickness 50.0 - 200 micronsRecommended
Melt Flow 0.50 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 95ISO 868/A
Hardness, Shore D 44ISO 868/A
Film Tensile Strength at Yield, MD 8.00 MPaISO 527-3
Film Tensile Strength at Yield, TD 8.00 MPaISO 527-3
Film Elongation at Break, MD 450 %ISO 527-3
Film Elongation at Break, TD 600 %ISO 527-3
Coefficient of Friction, Dynamic >= 0.20ISO 8295
Elmendorf Tear Strength, MD 2.6494 g/micronISO 6383-2
Elmendorf Tear Strength, TD 4.076 g/micronISO 6383-2
Dart Drop Test 420 gF50; ISO 7765-1
Film Tensile Strength at Break, MD 25.0 MPaISO 527-3
Film Tensile Strength at Break, TD 25.0 MPaISO 527-3
1% Secant Modulus, MD 120 MPaISO 527-3
1% Secant Modulus, TD 125 MPaISO 527-3
 
Thermal PropertiesOriginal ValueComments
Melting Point 104 °CInternal Method
Vicat Softening Point 85.0 °C
@Load 1.00 kg
ISO 306/A
Brittleness Temperature <= -80.0 °CASTM D746
 
Optical PropertiesOriginal ValueComments
Haze 6.0 %ISO 14782
Gloss 65 %45°; ASTM D2457

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Versalis Greenflex® FD 20 Ethylene Vinyl Acetate Copolymer - Blown Film Extrusion
Versalis Greenflex® FD 50 Ethylene Vinyl Acetate Copolymer - Blown Film Extrusion
Versalis Greenflex® FD 53 Ethylene Vinyl Acetate Copolymer - Blown Film Extrusion
Arkema Evatane® 1003 VL 2 Ethylene Vinyl Acetate
Arkema OREVAC® 18211 Maleic Anhydride Grafted EVA Copolymer

PENG135 / 124529

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.