MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Henkel Loctite® Stycast® 2057M with CAT 24LV Epoxy Encapsulant
Categories: Polymer; Thermoset; Epoxy; Epoxy Encapsulant, Unreinforced

Material Notes: Loctite Stycast 2057M provides the following product characteristics:
  • Low viscosity
  • Good machinability
  • General purpose
  • Rapid air release
  • Can be used with a variety of catalysts
  • Application: Encapsulation, Potting

Loctite Stycast 2057M is a general purpose encapsulant designed for machine dispensing and for parts requiring post molding machining. It contains a soft filler formulated to reduce abrasion in meter/mix equipment and to enhance machinability in the cured product.

Loctite Stycast 2057M can be used with a variety of catalysts.

CATALYST DESCRIPTION

Loctite CAT 24LV provides the following product characteristics:

  • Low color
  • Low viscosity
  • Long pot life
  • Excellent thermal shock and impact resistance
  • Excellent low temperature properties
  • Excellent adhesion to glass

Cure: Room temperature cure

Information provided by Henkel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³Part B, Loctite CAT 24LV
 1.74 g/cc0.0629 lb/in³Part A, Loctite Stycast 2057M
Water Absorption 0.63 %
@Temperature 100 °C,
Time 3600 sec
0.63 %
@Temperature 212 °F,
Time 1.00 hour
Cured
 0.22 %
@Time 86400 sec
0.22 %
@Time 24.0 hour
Cured, RT
 0.59 %
@Time 605000 sec
0.59 %
@Time 168 hour
7 Days at RT, Cured
Viscosity 35 cP35 cPPart B, Loctite CAT 24LV
Brookfield Viscosity 4.2 cP4.2 cPPart A, Loctite Stycast 2057M; Spindle 5, speed 50 rpm
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8787
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.10e+15 ohm-cm1.10e+15 ohm-cm
Surface Resistance 5.50e+16 ohm5.50e+16 ohm
Dielectric Constant  4.9
@Frequency 1e+6 Hz
4.9
@Frequency 1e+6 Hz
 5.3
@Frequency 50 Hz
5.3
@Frequency 50 Hz
 5.5
@Frequency 1000 Hz
5.5
@Frequency 1000 Hz
Dissipation Factor  0.0040
@Frequency 50 Hz
0.0040
@Frequency 50 Hz
 0.0080
@Frequency 1000 Hz
0.0080
@Frequency 1000 Hz
 0.039
@Frequency 1e+6 Hz
0.039
@Frequency 1e+6 Hz
 
Thermal PropertiesMetricEnglishComments
CTE, linear 137 µm/m-°C76.1 µin/in-°FAbove Tg
Maximum Service Temperature, Air 105 °C221 °FContinuous
 120 °C248 °FIntermittent
Minimum Service Temperature, Air -65.0 °C-85.0 °FContinuous
 -65.0 °C-85.0 °FIntermittent
Glass Transition Temp, Tg 38.0 °C100 °FTMA
 51.0 °C124 °FDMA, @ onset point
 63.0 °C145 °FDMA, tan delta
 
Processing PropertiesMetricEnglishComments
Cure Time  120 - 240 min
@Temperature 65.0 °C
2.00 - 4.00 hour
@Temperature 149 °F
Option 3
 360 - 480 min
@Temperature 45.0 °C
6.00 - 8.00 hour
@Temperature 113 °F
Option 2
 1440 min
@Temperature 25.0 °C
24.0 hour
@Temperature 77.0 °F
Option 1
Shelf Life 12.0 Month12.0 MonthPart A, Loctite Stycast 2057M
 
Descriptive Properties
AppearanceBlackPart A, Loctite Stycast 2057M
Mix Ratio, by Weight100 : 10Material : Catalyst

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PHENK7916 / 255403

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.