MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

Trinseo CALIBRE™ 2060-15 Polycarbonate, Sterilization Grade
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Unreinforced, Flame Retardant

Material Notes: CALIBRE® 2061-15 Polycarbonate resin is suitable for steam and ethylene oxide sterilization required by the health care industry. CALIBRE® 2061-15 provides exceptional clarity, heat resistance, impact strength, processability, and has low contamination levels. CALIBRE® 2061-15 resin is compliant with ISO 10993 (Biological Evaluation of Medical Devices) and is suitable for use in approved medical applications. This product contains mold release.

Main Characteristic:

  • Tested under ISO 10993
Application:
  • Medical applications

Data provided by Dow Chemical.

This product line was spun off from Dow Chemical to Styron in 2010.

Key Words: PC
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ASTM D792
Water Absorption 0.15 %0.15 %ASTM D570
Moisture Absorption at Equilibrium 0.32 %0.32 %ASTM D570
Linear Mold Shrinkage 0.0050 - 0.0070 cm/cm0.0050 - 0.0070 in/inFlow; ASTM D955
Melt Flow 15 g/10 min
@Load 1.20 kg,
Temperature 300 °C
15 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 7373ASTM D785
Hardness, Rockwell R 118118ASTM D785
Tensile Strength, Ultimate 68.3 MPa9910 psi50 mm/min; ASTM D638
Tensile Strength, Yield 62.1 MPa9010 psi50 mm/min; ASTM D638
Elongation at Break 150 %150 %50 mm/min; ASTM D638
Elongation at Yield 6.0 %6.0 %50 mm/min; ASTM D638
Tensile Modulus 2.34 GPa339 ksi50 mm/min; ASTM D638
Flexural Strength 96.5 MPa14000 psiMethod I (3 point), 2.0 mm/min; ASTM D790
 98.0 MPa14200 psi2.0 mm/min; ISO 178
Flexural Modulus 2.40 GPa348 ksi2.0 mm/min; ISO 178
 2.41 GPa350 ksiMethod I (3 point), 2.0 mm/min; ASTM D790
Izod Impact, Notched 7.50 J/cm14.1 ft-lb/inASTM D256
Izod Impact, Unnotched NBNBASTM D256
Izod Impact, Notched (ISO) 74.0 kJ/m²35.2 ft-lb/in²ISO 180/A
Charpy Impact, Notched 2.50 J/cm²11.9 ft-lb/in²ISO 179/1eA
Tensile Impact Strength 378 kJ/m²180 ft-lb/in²ASMT D1822
Instrumented Impact Total Energy 81.3 J
@Temperature 23.0 °C
60.0 ft-lb
@Temperature 73.4 °F
ASMT D3763
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 2.00e+17 ohm-cm2.00e+17 ohm-cmASTM D257
Dielectric Constant  3.0
@Frequency 60 Hz
3.0
@Frequency 60 Hz
ASTM D149
 3.0
@Frequency 1e+6 Hz
3.0
@Frequency 1e+6 Hz
ASTM D149
Dielectric Strength 17.0 kV/mm432 kV/inASTM D150
Dissipation Factor  0.00010
@Frequency 60 Hz
0.00010
@Frequency 60 Hz
ASTM D149
 0.0020
@Frequency 1e+6 Hz
0.0020
@Frequency 1e+6 Hz
ASTM D149
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 68.0 µm/m-°C
@Temperature -40.0 - 82.0 °C
37.8 µin/in-°F
@Temperature -40.0 - 180 °F
ASTM D696
Deflection Temperature at 1.8 MPa (264 psi) 120 °C248 °FUnannealed; ISO 75-2/A
 122 °C252 °FUnannealed; ASTM D648
 122 °C252 °FUnannealed; ASTM D648
 136 °C277 °FAnnealed; ASTM D648
Vicat Softening Point 143 °C289 °FISO 306/B50
 148 °C298 °FRate A (50°C), Loading 2 (50N); ASTM D1525
Flammability, UL94  HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
 HB
@Thickness 3.00 mm
HB
@Thickness 0.118 in
 V-2
@Thickness 1.50 mm
V-2
@Thickness 0.0591 in
 V-2
@Thickness 0.750 mm
V-2
@Thickness 0.0295 in
Oxygen Index 26 %26 %
 
Optical PropertiesMetricEnglishComments
Refractive Index 1.5861.586ASTM D542
Haze 1.0 %1.0 %ASTM D1003
Transmission, Visible 89 %89 %ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polycarbonate/ABS Alloy, Unreinforced
Trinseo CALIBRE™ 2061-15 Polycarbonate Resin
Trinseo EMERGE™ 7700 Polycarbonate (PC) / Acrylonitrile Butadiene Styrene (ABS)
Trinseo EMERGE™ 9500CR Polycarbonate (PC) / Polyethylene Terephthalate (PET)
Dow Tyril® 100 SAN

PZZDW020 / 34251

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.