MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Teknor Apex Telcar® TL-86-K902A Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Telcar TL-86-K902A is a general purpose thermoplastic elastomer designed for the industrial market. Telcar TL-86-K902A is high density, medium hardness grade suitable for both injection molding and extrusion.

Features: Filled; High Density; High Specific Gravity; Light Stabilized; Low Flow; Medium Hardness; Slip

Uses: Building Materials; Glazing; Industrial Applications; Windows & Doors

Form: Pellets

Processing Method: Injection Molding; Extrusion

Injection Notes: Injection Rate: Moderate-Fast

Extrusion Notes: Screw Speed: 30 to 100 rpm

Information Provided by Teknor Apex

Key Words: TPE
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.18 g/ccASTM D792
Melt Flow 0.40 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 75
@Time 15.0 sec
ASTM D2240
 77
@Time 1.00 sec
ASTM D2240
Tensile Strength at Break 6.17 MPaFlow, Die C, 20 in/min; ASTM D412
 1570 psiAcross Flow, Die C, 20 in/min; ASTM D412
Tensile Stress at Strain 392 psi
@Strain 100 %
Across Flow, Die C, 20 in/min; ASTM D412
 568 psi
@Strain 300 %
Across Flow, Die C, 20 in/min; ASTM D412
 770 psi
@Strain 100 %
Flow, Die C, 20 in/min; ASTM D412
Elongation at Break 280 %Flow, Die C, 20 in/min; ASTM D412
 710 %Across Flow, Die C, 20 in/min; ASTM D412
Tear Strength 191 pliFlow, Die C, 20 in/min; ASTM D624
 215 pliAcross Flow, Die C, 20 in/min; ASTM D624
Compression Set 25 %
@Temperature 22.8 °C,
Time 79200 sec
Type 1; ASTM D395B
 46 %
@Temperature 70.0 °C,
Time 79200 sec
Type 1; ASTM D395B
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 340 - 380 °F
Middle Barrel Temperature 350 - 390 °F
Front Barrel Temperature 360 - 400 °F
Nozzle Temperature 370 - 410 °F
Zone 1 330 - 370 °F
Zone 2 340 - 380 °F
Zone 3 350 - 390 °F
Zone 5 360 - 400 °F
Die Temperature 374 - 410 °F
Melt Temperature 370 - 410 °FProcessing Temperature
Mold Temperature 77.0 - 150 °F
Injection Pressure 200 - 1000 psi
Back Pressure 25.0 - 50.0 psi
Cushion 0.150 - 1.00 in
Screw Speed 50 - 100 rpm
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNP525 / 129606

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.