MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Envalior Durethan® BKV 15 H.3 DUS008 000000 Nylon 6, 15% Glass Fiber
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 20% Glass Fiber Filled; Nylon 6, Heat Stabilized

Material Notes: PA 6, 15% glass fibers, injection molding, heat-ageing stabilized

Former Lanxess product line is now with Envalior.

Key Words: ISO 1874-PA6, GHR,14-070,GF15
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.228 g/cc0.04436 lb/in³ISO 1183
Linear Mold Shrinkage, Flow 0.0035 cm/cm0.0035 in/in150x105x3, 280°C / MT 80°C; 500 bar; ISO 2577
Linear Mold Shrinkage, Transverse 0.0060 cm/cm0.0060 in/in150x105x3, 280°C / MT 80°C; 500 bar; ISO 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 65.0 MPa9430 psiconditioned, 5 mm/min; ISO 527-1,-2
 130 MPa18900 psi5 mm/min; ISO 527-1,-2
Elongation at Break 3.0 %3.0 %5 mm/min; ISO 527-1,-2
 12 %12 %conditioned, 5 mm/min; ISO 527-1,-2
Tensile Modulus 3.10 GPa450 ksiconditioned, 1 mm/min; ISO 527-1,-2
 6.50 GPa943 ksi1 mm/min; ISO 527-1,-2
Flexural Strength 110 MPa16000 psiconditioned, 2 mm/min; ISO 178-A
 205 MPa29700 psi2 mm/min; ISO 178-A
Flexural Modulus 3.10 GPa450 ksiconditioned, 2 mm/min; ISO 178-A
 5.50 GPa798 ksi2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)  <= 10.0 kJ/m²
@Temperature 23.0 °C
<= 4.76 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1A
 10.0 kJ/m²
@Temperature 23.0 °C
4.76 ft-lb/in²
@Temperature 73.4 °F
conditioned; ISO 180-1A
Izod Impact, Unnotched (ISO)  40.0 kJ/m²
@Temperature -30.0 °C
19.0 ft-lb/in²
@Temperature -22.0 °F
ISO 180-1U
 40.0 kJ/m²
@Temperature -30.0 °C
19.0 ft-lb/in²
@Temperature -22.0 °F
conditioned; ISO 180-1U
 45.0 kJ/m²
@Temperature 23.0 °C
21.4 ft-lb/in²
@Temperature 73.4 °F
ISO 180-1U
 85.0 kJ/m²
@Temperature 23.0 °C
40.4 ft-lb/in²
@Temperature 73.4 °F
conditioned; ISO 180-1U
Charpy Impact Unnotched  4.50 J/cm²
@Temperature -30.0 °C
21.4 ft-lb/in²
@Temperature -22.0 °F
ISO 179-1eU
 4.50 J/cm²
@Temperature -30.0 °C
21.4 ft-lb/in²
@Temperature -22.0 °F
conditioned; ISO 179-1eU
 5.00 J/cm²
@Temperature 23.0 °C
23.8 ft-lb/in²
@Temperature 73.4 °F
ISO 179-1eU
 10.0 J/cm²
@Temperature 23.0 °C
47.6 ft-lb/in²
@Temperature 73.4 °F
conditioned; ISO 179-1eU
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 30.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
16.7 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
CTE, linear, Transverse to Flow 100 µm/m-°C
@Temperature 23.0 - 55.0 °C
55.6 µin/in-°F
@Temperature 73.4 - 131 °F
ISO 11359-1,-2
Melting Point 220 °C428 °F10°C/min; ISO 11357-1,-3
Deflection Temperature at 0.46 MPa (66 psi) 215 °C419 °FISO 75-1,-2
Deflection Temperature at 1.8 MPa (264 psi) 195 °C383 °FISO 75-1,-2
Shrinkage  0.15 %
@Temperature 120 °C,
Time 14400 sec
0.15 %
@Temperature 248 °F,
Time 4.00 hour
post-shrinkage, 150x105x3; ISO 2577
 0.15 %
@Temperature 120 °C,
Time 14400 sec
0.15 %
@Temperature 248 °F,
Time 4.00 hour
post-shrinkage, transverse, 150x105x3; ISO 2577
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 °C536 °FInjection molding; ISO 294
Mold Temperature 80.0 °C176 °FInjection molding; ISO 294
Dry Time 2.00 - 6.00 hour
@Temperature 80.0 °C
2.00 - 6.00 hour
@Temperature 176 °F
Moisture Content 0.030 - 0.12 %0.030 - 0.12 %residual; Karl Fischer test

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chi Mei Polylac® PA-777E ABS - High Heat
Chi Mei Polylac® PA-777D ABS - High Heat
Chi Mei Polylac® PA-777B ABS - High Heat
Overview of materials for Polycarbonate/Polybutylene Terephthalate (PBT) Blend, Glass Filled
Envalior Arnite® TV4 461 (PBT+PET)-GF30

PLANX0501 / 150460

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.