Physical Properties | Metric | English | Comments |
---|
Specific Gravity | 1.46 g/cc | 1.46 g/cc |
Density | 1.46 g/cc | 0.0527 lb/in³ |
Filler Content | 30 % | 30 % |
Water Absorption | 0.71 % | 0.71 % |
Moisture Absorption | 0.230 % | 0.230 % |
Viscosity | 130 cP @Shear Rate 1500 1/s, Temperature 260 °C | 130 cP @Shear Rate 1500 1/s, Temperature 500 °F |
Linear Mold Shrinkage, Flow | 0.0010 - 0.0030 cm/cm | 0.0010 - 0.0030 in/in |
| 0.0030 - 0.0070 cm/cm @Thickness 3.20 mm | 0.0030 - 0.0070 in/in @Thickness 0.126 in |
Linear Mold Shrinkage, Transverse | 0.0030 - 0.0070 cm/cm | 0.0030 - 0.0070 in/in |
Melt Flow | 13 g/10 min @Load 3.80 kg, Temperature 200 °C | 13 g/10 min @Load 8.38 lb, Temperature 392 °F |
| 13 g/10 min @Load 5.00 kg, Temperature 250 °C | 13 g/10 min @Load 11.0 lb, Temperature 482 °F |
| 25 g/10 min @Load 5.00 kg, Temperature 265 °C | 25 g/10 min @Load 11.0 lb, Temperature 509 °F |
| 35 g/10 min @Load 5.00 kg, Temperature 266 °C | 35 g/10 min @Load 11.0 lb, Temperature 511 °F |
| 35 g/10 min @Load 5.00 kg, Temperature 265 °C | 35 g/10 min @Load 11.0 lb, Temperature 509 °F |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell R | 116 | 116 |
Ball Indentation Hardness | 210 MPa | 30500 psi |
Tensile Strength at Break | 125 MPa | 18100 psi |
| 130 MPa | 18900 psi |
Tensile Strength, Yield | 125 MPa | 18100 psi |
| 130 MPa | 18900 psi |
Elongation at Break | 2.8 % | 2.8 % |
| 2.8 % | 2.8 % |
Elongation at Yield | 2.8 % | 2.8 % |
| 2.8 % | 2.8 % |
Tensile Modulus | 9.50 GPa | 1380 ksi |
| 9.60 GPa | 1390 ksi |
Flexural Strength | 180 MPa | 26100 psi |
Flexural Yield Strength | 175 MPa | 25400 psi |
| 185 MPa | 26800 psi |
Flexural Modulus | 7.70 GPa | 1120 ksi |
| 8.20 GPa | 1190 ksi |
Flexural Strain at Break | 2.9 % | 2.9 % |
Izod Impact, Notched | 0.800 J/cm | 1.50 ft-lb/in |
| 0.800 J/cm @Temperature -30.0 °C | 1.50 ft-lb/in @Temperature -22.0 °F |
| 0.800 J/cm @Temperature 0.000 °C | 1.50 ft-lb/in @Temperature 32.0 °F |
Izod Impact, Unnotched | 8.00 J/cm | 15.0 ft-lb/in |
| 8.00 J/cm @Temperature -30.0 °C | 15.0 ft-lb/in @Temperature -22.0 °F |
Izod Impact, Notched (ISO) | 9.00 kJ/m² | 4.28 ft-lb/in² |
| 8.00 kJ/m² @Temperature -30.0 °C | 3.81 ft-lb/in² @Temperature -22.0 °F |
| 8.00 kJ/m² @Temperature 0.000 °C | 3.81 ft-lb/in² @Temperature 32.0 °F |
Izod Impact, Unnotched (ISO) | 50.0 kJ/m² | 23.8 ft-lb/in² |
| 45.0 kJ/m² @Temperature -30.0 °C | 21.4 ft-lb/in² @Temperature -22.0 °F |
Charpy Impact Unnotched | 3.00 J/cm² | 14.3 ft-lb/in² |
| 5.50 J/cm² | 26.2 ft-lb/in² |
| 2.50 J/cm² @Temperature -30.0 °C | 11.9 ft-lb/in² @Temperature -22.0 °F |
| 4.50 J/cm² @Temperature -30.0 °C | 21.4 ft-lb/in² @Temperature -22.0 °F |
Charpy Impact, Notched | 0.700 J/cm² | 3.33 ft-lb/in² |
| 0.900 J/cm² | 4.28 ft-lb/in² |
| 0.600 J/cm² @Temperature -30.0 °C | 2.86 ft-lb/in² @Temperature -22.0 °F |
| 0.900 J/cm² @Temperature -30.0 °C | 4.28 ft-lb/in² @Temperature -22.0 °F |
Dart Drop, Total Energy | 78.0 J | 57.5 ft-lb |
Taber Abrasion, mg/1000 Cycles | 65 | 65 |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | >= 1.00e+15 ohm-cm | >= 1.00e+15 ohm-cm |
Surface Resistance | >= 1.00e+15 ohm | >= 1.00e+15 ohm |
Dielectric Constant | 3.2 @Frequency 1e+6 Hz | 3.2 @Frequency 1e+6 Hz |
| 3.6 @Frequency 50.0 - 60.0 Hz | 3.6 @Frequency 50.0 - 60.0 Hz |
Dielectric Strength | 21.0 kV/mm @Thickness 3.20 mm | 533 kV/in @Thickness 0.126 in |
Dissipation Factor | 0.0024 @Frequency 50.0 - 60.0 Hz | 0.0024 @Frequency 50.0 - 60.0 Hz |
| 0.0182 @Frequency 1e+6 Hz | 0.0182 @Frequency 1e+6 Hz |
Comparative Tracking Index | 400 - 600 V | 400 - 600 V |
| 500 V | 500 V |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear, Parallel to Flow | 22.0 µm/m-°C @Temperature -40.0 - 40.0 °C | 12.2 µin/in-°F @Temperature -40.0 - 104 °F |
| 22.0 µm/m-°C @Temperature 23.0 - 60.0 °C | 12.2 µin/in-°F @Temperature 73.4 - 140 °F |
CTE, linear, Transverse to Flow | 115 µm/m-°C @Temperature -40.0 - 40.0 °C | 63.9 µin/in-°F @Temperature -40.0 - 104 °F |
| 115 µm/m-°C @Temperature 23.0 - 60.0 °C | 63.9 µin/in-°F @Temperature 73.4 - 140 °F |
Thermal Conductivity | 0.260 W/m-K | 1.80 BTU-in/hr-ft²-°F |
Hot Ball Pressure Test | 125 °C | 257 °F |
Deflection Temperature at 0.46 MPa (66 psi) | 215 °C | 419 °F |
Deflection Temperature at 1.8 MPa (264 psi) | 190 °C | 374 °F |
| 190 °C @Thickness 3.20 mm | 374 °F @Thickness 0.126 in |
Vicat Softening Point | 182 °C | 360 °F |
| 182 °C | 360 °F |
| 182 °C | 360 °F |
| 218 °C | 424 °F |
| 218 °C | 424 °F |
UL RTI, Electrical | 50.0 °C | 122 °F |
UL RTI, Mechanical with Impact | 50.0 °C | 122 °F |
UL RTI, Mechanical without Impact | 50.0 °C | 122 °F |
Flammability, UL94 | HB @Thickness 0.750 mm | HB @Thickness 0.0295 in |
| HB @Thickness 3.00 mm | HB @Thickness 0.118 in |
Glow Wire Test | 750 °C @Thickness 1.00 mm | 1380 °F @Thickness 0.0394 in |
|
Processing Properties | Metric | English | Comments |
---|
Processing Temperature | 40.0 - 60.0 °C | 104 - 140 °F |
Nozzle Temperature | 240 - 260 °C | 464 - 500 °F |
Zone 1 | 230 - 245 °C | 446 - 473 °F |
Zone 2 | 240 - 255 °C | 464 - 491 °F |
Zone 3 | 245 - 265 °C | 473 - 509 °F |
Melt Temperature | 250 - 270 °C | 482 - 518 °F |
Mold Temperature | 40.0 - 100 °C | 104 - 212 °F |
Drying Temperature | 110 - 120 °C | 230 - 248 °F |
Dry Time | 2.00 - 4.00 hour | 2.00 - 4.00 hour |
Moisture Content | 0.020 % | 0.020 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.