MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Braskem Flexus® 9211 LLDPE Blow Film Extrusion Polyethylene Copolymer  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE); Linear Low Density Polyethylene (LLDPE), Film Grade; LLDPE/Hexene, Film Grade

Material Notes: Braskem Flexus 9211 is a LLDPE hexene copolymer produced through a metallocene catalyst, which presents excellent impact and puncture strength beyond a differential sealing performance compared with another typical LLDPE. It contains medium slip, medium blocking, and medium level processing aid additives. Its applications include: automatic packaging (FFS), multilayer packaging films, and films for lamination.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.917 g/ccASTM-D792
Melt Flow 1.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM-D1238
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 850 %ASTM-D882
Film Elongation at Break, TD 840 %ASTM-D882
Elmendorf Tear Strength MD 230 gASTM-D1922
Elmendorf Tear Strength TD 790 gASTM-D1922
Dart Drop Test >= 850 gASTM-D1709
Film Tensile Strength at Break, MD 35.0 MPaASTM-D882
Film Tensile Strength at Break, TD 25.0 MPaASTM-D882
1% Secant Modulus, MD 150 MPaASTM-D882
1% Secant Modulus, TD 160 MPaASTM-D882
 
Optical PropertiesOriginal ValueComments
Haze 7.0 %ASTM-D1003
Gloss 84 %Angle 60°; ASTM-D2457

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Petroquimica Triunfo Trithene® TS 7006 LDPE - Coextruded Film
Nabaltec GRANALOX® NM 9212 E Ceramic Bodies
Braskem EB853/72 Blown Film Extrusion Low Density Polyethylene
Braskem LH218 Cast Film Extrusion Linear Low Density Polyethylene
Braskem HC7260LS-L HDPE Injection Molding Polyethylene

PBRAS856 / 106702

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.