MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
LG Chemical ABS-AF-315 ABS Flame Retardant ABS Resin  (discontinued **)
Categories: Polymer; Thermoplastic; ABS Polymer; Acrylonitrile Butadiene Styrene (ABS), Unreinforced, Flame Retardant

Material Notes: Information provided by US distributor Polymer Technology and Services, LLC (PTS).

Key Words: Poly(Acrylonitrile Butadiene Styrene)
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.21 g/ccASTM D792
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cmASTM D955
Melt Flow 35 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 104ASTM D785
Tensile Strength, Yield 44.0 MPa50 mm/min; ASTM D638
Elongation at Break 25 %50 mm/min; ASTM D638
Flexural Yield Strength 77.0 MPa50 mm/min; ASTM D790
Flexural Modulus 2.30 GPa15 mm/min; ASTM D790
Izod Impact, Notched 1.04 J/cm
@Thickness 6.35 mm
ASTM D256
 1.65 J/cm
@Thickness 3.17 mm
ASTM D256
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 83.0 °C
@Thickness 6.35 mm
Unannealed; ASTM D648
Flammability, UL94 V-0
@Thickness 1.59 mm
 V-0
@Thickness 3.17 mm
V-0/5V
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 350 °F
Middle Barrel Temperature 400 °F
Front Barrel Temperature 420 °F
Melt Temperature 450 - 480 °FNozzle temp not greater than stock
Mold Temperature 130 - 160 °F
Drying Temperature 190 - 200 °F
Dry Time 2 - 24 hour
Injection Pressure 8000 - 12000 psi
Back Pressure 100 psi
Screw Speed 50 - 60 rpm
 
Descriptive Properties
Injection Fill SpeedSlow to Moderate

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Samyang Trirex® 3500G20 Polycarbonate, 20% Glass Reinforced
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Sheet
Elix Polymers ELIX ABS L3FR Acrylonitrile Butadiene Styrene (ABS), Flame Retardant
Aurora Plastics AcryliMax 301HP ABS

PLAZ02 / 50261

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.