MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

3M 7904 Screen Printable Sheet Vinyl Label Material
Categories: Polymer; Adhesive

Material Notes: 3M™ Screen Printable Sheet Vinyl Label Material 7904 is a durable, high performance material that offers excellent conformability, good durability and moisture resistance. This label material utilizes 3M™ Adhesive 350, which is designed to permanently bond to high and low surface energy plastics, textured and contoured surfaces, powder coatings, and slightly oily metals.

Information provided by 3M

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Thickness 45.7 microns1.80 milAdhesive
 86.4 microns3.40 milFacestock
 170 microns6.70 milLiner
 
Mechanical PropertiesMetricEnglishComments
Peel Strength 0.0877 kN/m0.500 pliGlass, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.219 kN/m1.25 pliLD Polyethylene, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.219 kN/m1.25 pliLD Polyethylene, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.2410 kN/m1.375 pliPolycarbonate 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.2849 kN/m1.625 pliPolycarbonate 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.29582 kN/m1.6875 pliFinely Textured Powder Coating, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.307 kN/m1.75 pliFinely Textured Powder Coating, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.307 kN/m1.75 pliFinely Textured Powder Coating, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.3287 kN/m1.875 pliFinely Textured Powder Coating, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.351 kN/m2.00 pliLD Polyethylene, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.38347 kN/m2.1875 pliLD Polyethylene, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.40538 kN/m2.3125 pliGlass, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.40538 kN/m2.3125 pliHD Polyethylene, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.4163 kN/m2.375 pliFinely Textured Powder Coating, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.4163 kN/m2.375 pliLD Polyethylene, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.438 kN/m2.50 pliHD Polyethylene, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.44921 kN/m2.5625 pliFinely Textured Powder Coating, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.4602 kN/m2.625 pliLD Polyethylene, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.4602 kN/m2.625 pliFinely Textured Powder Coating, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.4602 kN/m2.625 pliSmooth Powder Coating, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.47112 kN/m2.6875 pliLD Polyethylene, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.47112 kN/m2.6875 pliPolypropylene, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.482 kN/m2.75 pliFinely Textured Powder Coating, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.482 kN/m2.75 pliPolypropylene, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.482 kN/m2.75 pliHD Polyethylene, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.49303 kN/m2.8125 pliSmooth Powder Coating, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.49303 kN/m2.8125 pliGlass, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.5040 kN/m2.875 pliStainless Steel, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.526 kN/m3.00 pliAluminum, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.53686 kN/m3.0625 pliSmooth Powder Coating, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.53686 kN/m3.0625 pliHD Polyethylene, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.5478 kN/m3.125 pliStainless Steel, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.5478 kN/m3.125 pliAluminum, 90° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.55877 kN/m3.1875 pliHD Polyethylene, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.570 kN/m3.25 pliGlass, 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.570 kN/m3.25 pliLD Polyethylene, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.58068 kN/m3.3125 pliPolypropylene, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.58068 kN/m3.3125 pliSmooth Powder Coating, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.60259 kN/m3.4375 pliSmooth Powder Coating, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.64642 kN/m3.6875 pliPolycarbonate 90° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.64642 kN/m3.6875 pliHD Polyethylene, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.64642 kN/m3.6875 pliPolypropylene, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.657 kN/m3.75 pliPolycarbonate 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.66833 kN/m3.8125 pliHD Polyethylene, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.66833 kN/m3.8125 pliPolypropylene, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.69024 kN/m3.9375 pliSmooth Powder Coating, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.69024 kN/m3.9375 pliStainless Steel, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.701 kN/m4.00 pliPolycarbonate 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.71216 kN/m4.0625 pliGlass, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.7231 kN/m4.125 pliPolypropylene, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.75598 kN/m4.3125 pliAluminum, 90° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.75598 kN/m4.3125 pliStainless Steel, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.75598 kN/m4.3125 pliAluminum, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.77789 kN/m4.4375 pliHD Polyethylene, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.789 kN/m4.50 pliGlass, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.79981 kN/m4.5625 pliStainless Steel, 90° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.8108 kN/m4.625 pliStainless Steel, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.8108 kN/m4.625 pliAluminum, 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.8108 kN/m4.625 pliAluminum, 180° Peel, Conditioned for 3 days at 49°C; ASTM D3330
 0.82172 kN/m4.6875 pliSmooth Powder Coating, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.833 kN/m4.75 pliPolypropylene, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.88746 kN/m5.0625 pliSmooth Powder Coating, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.8984 kN/m5.125 pliPolycarbonate 180° Peel, Initial, 10 min dwell at RT; ASTM D3330
 0.964 kN/m5.50 pliStainless Steel, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 0.97511 kN/m5.5625 pliAluminum, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.9861 kN/m5.625 pliPolycarbonate 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 0.9861 kN/m5.625 pliGlass, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 1.0189 kN/m5.8125 pliAluminum, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 1.0189 kN/m5.8125 pliStainless Steel, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 1.030 kN/m5.875 pliPolypropylene, 180° Peel, Conditioned for 24 hrs at 32°C at 90% RH; ASTM D3330
 1.0628 kN/m6.0625 pliPolycarbonate 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 1.074 kN/m6.125 pliGlass, 180° Peel, Conditioned for 3 days at RT; ASTM D3330
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 60.0 °C140 °F
Minimum Service Temperature, Air -40.0 °C-40.0 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature >= 5.00 °C>= 41.0 °FApplication
Shelf Life 24.0 Month24.0 Month
 
Descriptive Properties
Adhesive Type350 Acrylic
Liner90# Polyctd.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PMM33702 / 168449

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.