System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
Phillips 66 COPYLENE® CM100LN Polypropylene, Impact Copolymer, Medium Impact, Nucleated, Antistat, Injection Molding
(discontinued **)
Categories:
Polymer
;
Thermoplastic
;
Polypropylene (PP)
;
Polypropylene Copolymer
Material Notes:
Medium impact, nucleated, antistat, injection molding. Applications: Household articles, pails, consumer products.
Information provided by Phillips 66.
Key Words:
Medium impact, nucleated, antistat
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Metric
English
Comments
Density
0.902
g/cc
0.0326
lb/in³
ASTM D792
Melt Flow
10
g/10 min
@Load 2.16 kg,
Temperature 230 °C
10
g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Mechanical Properties
Metric
English
Comments
Tensile Strength, Yield
25.9
MPa
3750
psi
2 in/min; ASTM D638
Elongation at Yield
5.0 %
5.0 %
ASTM D638
Flexural Modulus, 1% Secant
1450
MPa
210000
psi
0.05 in/min; Procedure A; ASTM D790
Izod Impact, Notched
1.17
J/cm
@Temperature 23.0 °C
2.20
ft-lb/in
@Temperature 73.4 °F
Method A; ASTM D256
Thermal Properties
Metric
English
Comments
Deflection Temperature at 0.46 MPa (66 psi)
108
°C
226
°F
unannealed; ASTM D648
Descriptive Properties
Process
Injection Molding
**
Materials flagged as discontinued (
) are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.
Users of our Advanced Search (registration required) may exclude discontinued materials from search results.
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to view all the property values for this datasheet as they were originally entered into MatWeb.
Users viewing this material also viewed the following:
Phillips 66 COPYLENE® CM040LN Polypropylene, Impact Copolymer, Thermoforming
Phillips 66 COPYLENE® CM120LN Polypropylene Impact Copolymer
Phillips 66 COPYLENE® CM090L Polypropylene, High Impact Copolymer
Phillips 66 COPYLENE® CM020N Polypropylene Impact Copolymer
Phillips 66 COPYLENE® CM015G Polypropylene Impact Copolymer
PCOPY035 / 100831
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.