MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

E-Polymers TEKAMID® TA210HI , High Impact Resistance PA66, DAM
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: High impact resistance

Information provided by E-Polymers Co. Ltd.

Key Words: Polyamide 66
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.10 g/cc0.0397 lb/in³ASTM D792
Water Absorption 1.2 %1.2 %23°C/24 hr; ASTM D570
Linear Mold Shrinkage 0.015 cm/cm0.015 in/in
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 112112ASTM D786
Tensile Strength, Yield 67.0 MPa9720 psiASTM D638
Elongation at Break 60 %60 %ASTM D638
Flexural Yield Strength 95.0 MPa13800 psiASTM D790
Flexural Modulus 2.30 GPa334 ksiASTM D790
Izod Impact, Notched 3.00 J/cm5.62 ft-lb/inASTM D256
Izod Impact, Unnotched NB
@Thickness 3.20 mm
NB
@Thickness 0.126 in
ASTM D256
 
Thermal PropertiesMetricEnglishComments
CTE, linear 75.0 µm/m-°C
@Temperature 20.0 °C
41.7 µin/in-°F
@Temperature 68.0 °F
ASTM D696
Thermal Conductivity 0.250 W/m-K1.74 BTU-in/hr-ft²-°F
Melting Point 260 °C500 °FASTM D2133
Deflection Temperature at 0.46 MPa (66 psi) 225 °C437 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 80.0 °C176 °FASTM D648
Flammability, UL94 HBHB
 
Processing PropertiesMetricEnglishComments
Processing Temperature 270 - 290 °C518 - 554 °F
Mold Temperature 40.0 - 60.0 °C104 - 140 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
E-Polymers TEKAMID® H14ST Super Toughness PA/ABS Alloy
E-Polymers TEKAMID® TA210ST Super Tough PA66, DAM
Radici Radilon® A RV150 (cond.) Nylon 66
Eurotec® Tecomid® NA40 NL IX PA6.6, impact modified, natural
E-Polymers TEKAMID® TA210IR Impact Modified PA66 Resin

PEPOLY04 / 36306

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.