MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

RTP Company RTP 300 HF FR A UV Polycarbonate (PC), High Flow - Unreinforced - Flame Retardant - UV Stabilized - UL94 V-0
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Unreinforced, Flame Retardant

Material Notes: The RTP 300 FR A family of materials offer dimensional stability, rigidity, heat resistance, ignition resistance and excellent impact strength. RTP 300 HF FR A UV is a UV-stabilized, low viscosity grade which includes a UL94 5V-A certification.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.21 g/cc1.21 g/ccASTM D 792
Water Absorption 0.15 %0.15 %24 hrs @ 23°C; ASTM D 570
Linear Mold Shrinkage 0.0070 - 0.0090 cm/cm
@Thickness 3.17 mm
0.0070 - 0.0090 in/in
@Thickness 0.125 in
ASTM D955
Melt Flow 15 - 20 g/10 min
@Load 1.20 kg,
Temperature 300 °C
15 - 20 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ASTM D 1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 55.2 MPa8000 psiASTM D 638
Elongation at Break >= 10 %>= 10 %ASTM D 638
Tensile Modulus 2.28 GPa330 ksiASTM D 638
Flexural Strength 89.6 MPa13000 psiASTM D 790
Flexural Modulus 2.28 GPa330 ksiASTM D 790
Izod Impact, Notched 6.41 J/cm
@Thickness 3.17 mm
12.0 ft-lb/in
@Thickness 0.125 in
D 256
Izod Impact, Unnotched NB
@Thickness 3.17 mm
NB
@Thickness 0.125 in
ASTM D4812
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity >= 1.00e+16 ohm-cm>= 1.00e+16 ohm-cmASTM D 257
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 132 °C270 °FASTM D 648
Deflection Temperature at 1.8 MPa (264 psi) 127 °C260 °FASTM D 648
Flammability, UL94  V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in
 5VA
@Thickness 3.17 mm
5VA
@Thickness 0.125 in
 
Processing PropertiesMetricEnglishComments
Melt Temperature 288 - 316 °C550 - 600 °F
Mold Temperature 82.2 - 121 °C180 - 250 °F
Drying Temperature 121 °C250 °F
Dry Time 4 hour4 hour
Moisture Content 0.020 %0.020 %
Dew Point -28.9 °C-20.0 °F
Injection Pressure 68.9 - 103 MPa10000 - 15000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
RTP Company RTP 300 UV Polycarbonate (PC), UV Stabilized
RTP Company RTP 300 TFE 5 UV Polycarbonate (PC); PTFE Lubricated - UV Stabilized
RTP Company RTP 300 LF UV Polycarbonate (PC), Low Flow - UV Stabilized
RTP Company RTP 300 LF FR A UV Polycarbonate (PC), Low Flow - Unreinforced - Flame Retardant - UV Stabilized - UL94 V-0
RTP Company RTP 300 HF L UV Polycarbonate (PC), High Flow - Lubricated - UV Stabilized

PQZWA1135 / 90598

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.