MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Avient Polystrand ThermoPro™ IE6010 Unitape Unidirectional Polypropylene-Glass Composite  (discontinued **)
Categories: Polymer; Tape; Thermoplastic; Polypropylene (PP); Polypropylene with 60% Glass Fiber Filler

Material Notes: Fiber Orientation is 0°.

Polystrand ThermoPro™ combines continuous E-Glass (ThermoPro-E™) structural reinforcing fibers in either a polyethylene or polypropylene proprietary thermoplastic polymer to form ribbons or tapes. These material forms can be subsequently molded by high temperature processing to create end-use applications including pipe, tanks, liners, automotive, architectural, and a host of other structural industrial and commercial products. Polystrand ThermoPro™ is the result of a quest of more than 15-years to develop structural thermoplastic composites for the international industrial and commercial markets.

Information provided by Polystrand.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.50 g/cc
Filler Content 60 %E-Glass; ASTM D2584
Water Absorption 0.70 %ASTM D570
Thickness 330 microns
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 280 MPa0°; ASTM D3039
Elongation at Break 1.1 %0°; ASTM D3039
Tensile Modulus 25.1 GPa0°; ASTM D3039
Flexural Strength 420 MPa0°; measured on 0.1" panel molded from tape; ASTM D790
Flexural Modulus 24.1 GPa0°; measured on 0.1" panel molded from tape; ASTM D790
Shear Modulus 1.02 GPaIn-Plane G12; ASTM D5379
Shear Strength 24.8 MPaIn-Plane S12; ASTM D5379
 25.5 MPaInterlaminar S23; ASTM D2344
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.70 µm/m-°C
@Temperature 20.0 °C
Longitudinal; ASTM E228
CTE, linear, Transverse to Flow 64.6 µm/m-°C
@Temperature 20.0 °C
ASTM E228
Glass Transition Temp, Tg 165 °CASTM D3418

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Avient Polystrand ThermoPro™ IE7010 Unitape Unidirectional Polypropylene-Glass Composite
Reliance Industries METABOLIX PHB
Overview of materials for Polypropylene with 60% Glass Fiber Filler
PlastiComp Complet® LCF40 - PP Homopolymer Polypropylene, 40% Long Carbon Fiber Reinforced
Overview of materials for Acrylonitrile Butadiene Styrene (ABS), Molded

PPOLYST00 / 57668

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.