MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
ITW Devcon® Food Grade Pot & Seal
Categories: Polymer; Adhesive; Thermoset

Material Notes: Two-component adhesive for bonding aluminum, steel, stainless steel, and alloys of steel cloth. Approved for dry food contact. Uses: Bonding aluminum, stainless steel, and alloys of steel. Features: Excellent chemical, heat and water resistance, Thermal shock resistance.

Information provided by ITW Performance Polymers.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.0455 lb/in³
 10.5 lb/galuncured
Solids Content 100 %
Viscosity 100000 cPMixed
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 82
Elongation at Break 1.0 %
Izod Impact Resistance 5.20 ft-lb/in²
Peel Strength 2.00 - 3.00 pli
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 18.1 kV/mm
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 275 °F
Minimum Service Temperature, Air -40.0 °F
 
Processing PropertiesOriginal ValueComments
Cure Time 168 hour
@Temperature 24.0 °C
As Tested
 0.170 hour
@Pressure 13.4 MPa,
Temperature 93.0 °C
 0.250 hour
@Pressure 13.7 MPa,
Temperature 82.0 °C
Pot Life 42.0 min
@Temperature 22.2 °C
28gm
 
Descriptive Properties
Chemical/Solvent ResistanceAcetic (diluted) 10%: very good30 day immersion at 75°F. Sample cured 7 days at RT
 Ethanol: very good30 day immersion at 75°F. Sample cured 7 days at RT
 Glycols/Antifreeze: excellent30 day immersion at 75°F. Sample cured 7 days at RT
 Methanol: fair30 day immersion at 75°F. Sample cured 7 days at RT
 Motor Oil: excellent30 day immersion at 75°F. Sample cured 7 days at RT
 Sodium Hydroxide 10%: excellent30 day immersion at 75°F. Sample cured 7 days at RT
 Toluene: very good30 day immersion at 75°F. Sample cured 7 days at RT
 Xylene: excellent30 day immersion at 75°F. Sample cured 7 days at RT
ColorwhiteCured
Gap Filling (in)Excellent
Mix Ratio by volume4:1
Mix Ratio by weight100:25
Specific Volume (in.³/lb)22

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PITWD9217 / 239726

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.